WKZ002 / IE1006 Chemical Composition | WKZ566-2010
WKZ002 is the mill process-document identity used on this site for Caterpillar IE1006 / 1E1006 engineering-structure steel plate. The governing Chinese mill process scheme is WKZ566-2010 (effective 2010-08-26). Technology-department notice dated 2010-09-15 states that production must follow WKZ566-2010 strictly; the prior scheme WKZ036-2006 is void. This page focuses on grade identity, melting practice, and chemical composition (Table 1 plus internal-control Table 4). Mechanical properties and rolling/inspection practice are covered on the companion process page.
WKZ002 / IE1006 Identity under WKZ566-2010
Scope: plates for Caterpillar 1E1006 engineering structures with thickness not exceeding 100 mm. Dimensions, shape, weight and tolerances follow ASTM A6. Flatness shall not exceed 4 mm/m, and the number of waves per 4 m shall not exceed 3. Delivery condition is hot-rolled. Melting route is electric-arc furnace plus secondary refining; the steel is aluminum fine-grain killed.
On mill certificates and spray marks the technical condition is named bilingually as Caterpillar 1E1006. Do not confuse the mill process code WKZ002 / WKZ566-2010 with a public ASTM grade number; buyer documents should cite Caterpillar 1E1006 (IE1006) together with the applicable mill process edition.
Chemical Composition — Heat Analysis (Table 1, WKZ566-2010)
Table 1 heat-analysis limits (wt%) for 1E1006 / IE1006 plate under WKZ566-2010:
| Element |
C |
Si |
Mn |
P |
S |
Al |
Nb |
V |
Ti |
| Content |
≤0.20 |
≤0.55 |
≤1.60 |
≤0.025 |
≤0.035 |
≥0.020 |
≤0.05 |
≤0.15 |
≤0.05 |
Combined microalloy limit: Nb + V ≤ 0.15%. Heat analysis on the MTC must meet Table 1; product acceptance still follows the ordered Caterpillar / mill edition.
Internal Chemical Control (Table 4 by Thickness)
WKZ566-2010 Table 4 tightens melting practice with standard / internal-control / target rows split at 25 mm thickness. Steelmaking is judged against the internal-control band; the upper limit of Al may be relaxed to 0.060%.
| Thickness |
Category |
C |
Si |
Mn |
P |
S |
Nb |
V |
Al |
| All |
Standard (Table 1) |
≤0.20 |
≤0.55 |
≤1.60 |
≤0.025 |
≤0.035 |
Nb+V ≤0.15 |
≥0.020 |
| <25 mm |
Internal control |
0.16–0.18 |
0.15–0.25 |
1.50–1.60 |
≤0.015 |
≤0.003 |
0.030–0.035 |
0.055–0.060 |
0.020–0.040 |
| Target |
0.17 |
0.20 |
1.55 |
0.010 |
0.002 |
0.032 |
0.057 |
0.030 |
| ≥25 mm |
Internal control |
0.16–0.18 |
0.35–0.45 |
1.50–1.60 |
≤0.015 |
≤0.003 |
0.030–0.035 |
0.065–0.070 |
0.020–0.040 |
| Target |
0.17 |
0.40 |
1.55 |
0.010 |
0.002 |
0.032 |
0.068 |
0.030 |
Melting and Refining Notes Linked to Chemistry
Process flow for chemistry control: EAF → LF → VD → continuous casting. Prefer refined scrap; briquettes, slag steel, ladle-bottom residue and scrap moulds are excluded. Do not melt this grade in the first two heats after a new furnace body, new furnace lid or new ladle, or under abnormal furnace conditions. Ladle bake ≥ 900 °C. Slag-free tap with [C] ≤ 0.10%, [P] ≤ 0.008%, tap temperature 1620–1660 °C. Vacuum treatment: vacuum ≤ 66 Pa for ≥ 15 min with stable argon stirring. Continuous casting follows the mill WH60A-related rules; do not cast continuously with lower-strength grades (same-level grades such as SM570 / WH60 / S460 are permitted with extra transition-slab cutting).
Frequently Asked Questions
What is WKZ002 / IE1006 Steel Plate Chemical Composition under WKZ566-2010?
It is the heat-analysis package for Caterpillar 1E1006 / IE1006 plate as locked in mill process document WKZ566-2010 (site filename WKZ002). Table 1 gives the contractual maxima/minima; Table 4 is the mill internal-control band used in steelmaking.
How do Table 1 and Table 4 differ on the WKZ002 / IE1006 chemistry page?
Table 1 is the published specification limit set (for example C ≤ 0.20, P ≤ 0.025). Table 4 splits <25 mm and ≥25 mm and sets narrower internal-control and target windows so mechanical scatter is reduced. Heat release is judged to the internal-control row.
Why does WKZ002 cite WKZ566-2010 instead of WKZ036-2006?
The 2010-09-15 technology notice voids WKZ036-2006 and requires strict execution of WKZ566-2010 after quality fluctuations on Caterpillar 1E1006 plate. Certificates and RFQs should name the current edition.
What melting route supports the WKZ002 / IE1006 chemical composition?
Electric furnace melting with LF secondary refining and VD vacuum degassing, aluminum fine-grain killed, delivered hot-rolled. Vacuum hold ≤66 Pa for at least 15 minutes is part of the chemistry/cleanliness package.
Does Nb + V ≤ 0.15% apply together with individual Nb, V and Ti caps?
Yes. Individual limits are Nb ≤ 0.05, V ≤ 0.15 and Ti ≤ 0.05, and the combined Nb + V sum must also stay ≤ 0.15%. Check both the individual and combined lines on the MTC.
How should buyers RFQ WKZ002 / IE1006 chemistry with Gangsteel?
State Caterpillar 1E1006 (IE1006), thickness × width × length, quantity, hot-rolled delivery, required certificate language, and that chemistry must meet WKZ566-2010 Table 1 (and any agreed internal-control extras). See also the mechanical/process companion page for tensile and rolling notes. Contact Gangsteel for mill options.
Related Process Page
For transverse mechanical properties (Table 2), controlled-rolling temperatures, surface limits, inspection to A6/A370 and packaging to GB/T 247—1997, see WKZ002 / IE1006 Mechanical Properties & Process | WKZ566-2010.