EN 10083-3 Alloy Steel Plate

EN10083-3 30MnB5 STEEL PLATE

Gangsteel (HENAN GANG IRON AND STEEL CO.,LTD.) supplies EN 10083-3 30MnB5 (steel number 1.5531) as hot-rolled plate for parts that are cut, machined and then quenched and tempered. EN 10083-3:2006 classifies 30MnB5 as a boron-alloyed manganese steel for quenching and tempering: C 0.27–0.33%, Mn 1.15–1.45%, boron 0.0008–0.0050%. It raises the carbon of 20MnB5 to give higher as-quenched hardness, while keeping boron for hardenability and remaining shearable untreated. This page sets out the chemistry, the quenched and tempered property table, the Jominy hardenability band, delivery conditions and heat treatment guidance from the standard, so that a purchase order can name exactly what is needed.

What is EN 10083-3 30MnB5?

EN 10083-3 is Part 3 of the European standard for steels for quenching and tempering and covers the alloy grades (Part 2 covers the non-alloy grades). Its scope includes semi-finished products, bars, rod, wide flats, forgings and hot-rolled strip and sheet/plate. All grades are special steels; the standard requires a fine austenite grain size of 5 or finer and a special-steel level of cleanness. 30MnB5 indicates about 0.30% mean carbon; the suffix 5 refers to manganese divided by the factor 4, about 1.25% Mn, and B shows that boron is added. The steel number 1.5531 identifies the same grade in the EN 10027-2 numbering system.

The grade can be ordered with or without hardenability requirements. Without a suffix, the order is governed by the chemical composition and the mechanical properties after quenching and tempering. With the suffix +H, the Jominy hardenability band of Table 5 becomes a requirement. Either way, the steel is designed to be hardened by the user; plate in the as-rolled condition does not yet have the tabulated strength.

30MnB5 Chemical Composition (EN 10083-3:2006 Table 3)

Table 3 gives the cast analysis. The ranges below are those printed for 30MnB5 (1.5531); elements not quoted may not be added intentionally without the purchaser’s agreement, except for finishing the heat and for boron to have its effect.

Grade (number)C %Si %Mn %P %S %B %
30MnB5 (1.5531)0.27–0.33≤ 0.401.15–1.45≤ 0.025≤ 0.0350.0008–0.0050

Product (check) analysis may deviate from the cast analysis by the amounts in Table 4. For this grade the relevant permissible deviations are:

ElementCast analysis, %Permissible deviation, %
C0.27–0.33±0.02
Si≤ 0.40+0.03
Mn1.15–1.45±0.05
P≤ 0.025+0.005
S≤ 0.035+0.005
B0.0008–0.0050±0.0003

Notes: deviations in product analysis apply to individual elements; within one cast, the deviation of an element may lie above the upper limit or below the lower limit of the Table 3 range, but not both at the same time. Footnote c to Table 3, which allows sulphur up to about 0.10% by agreement for machinability, is printed for the steels without boron and does not apply to this boron grade. Boron in the range 0.0008–0.0050% is specified to raise hardenability; the standard permits the additions needed for boron to have its effect.

30MnB5 Mechanical Properties, Quenched and Tempered (+QT, Table 8)

Table 8 gives minimum yield strength, the tensile strength range, elongation, reduction of area and Charpy V-notch energy for 30MnB5 after quenching and tempering, listed by ruling section. For flat products the ruling section is the thickness t; the round-bar diameter d of the same column is shown for comparison. For 30MnB5, values are tabulated up to t ≤ 20 mm.

Plate thickness t, mmBar diameter d, mmRe min, MPaRm, MPaA min, %Z min, %KV min, J
t ≤ 8d ≤ 16800950–11501350–
8 < t ≤ 2016 < d ≤ 40650800–950135060

Notes: Re is the upper yield strength or, where no yield phenomenon occurs, the 0.2% proof strength Rp0.2. Impact values are not specified for the thinnest ruling section. The original page lists plate up to 300 mm thick; Table 8 stops at t ≤ 20 mm for this grade, so for thicker plate the mechanical requirements must be agreed for the actual product at the time of order. Not all flat-product dimensions can be supplied in the +QT condition.

30MnB5+H Hardenability Band (Jominy, Table 5)

The end-quench (Jominy) test according to EN ISO 642 measures how hardness falls with distance from the water-quenched end of a standard bar. For 30MnB5+H the test is carried out from 880 °C, and the measured hardness must stay within the band below. The band describes the steel’s capacity to harden; it is the most direct way to check whether a cast will through-harden in a given section.

Distance from quenched end, mmHRC maxHRC min
1.55647
35546
55545
75444
95342
115139
135036
154731
204022
2537–
3033–
35––
40––
45––
50––

Notes: a dash means no limit is set at that distance. The values apply to the +H grade only; a grade ordered without +H is not tested against the band. Annex C (Table C.1) gives guidance on the largest round diameters that reach 40 HRC in the core after hardening from 880 °C: about 38 mm when quenched in water and 30 mm in oil.

30MnB5 Delivery Condition

Table 1 of EN 10083-3 lists the heat treatment conditions in which products can be delivered. If nothing is agreed, the steel is supplied untreated, i.e. as hot rolled. For plate in 30MnB5 the usual choices are untreated (for later quenching and tempering by the fabricator), a condition that eases shearing and machining, or quenched and tempered to a Table 8 property class.

ConditionSymbolRequirement for 30MnB5
Untreatednone or +UDefault when not agreed; as-rolled, for heat treatment by the user
Treated to improve shearability+SNot specified; shearable in the untreated condition (7.3.3)
Soft annealed+ANot applicable to boron steels
Quenched and tempered+QTTable 8 properties for the ordered thickness
Otherby agreemente.g. annealing to a certain structure, agreed at enquiry and order

Notes: for the untreated, +S and +A conditions the Table 8 properties must still be achievable after correct quenching and tempering. 30MnB5 is listed in 7.3.3 as shearable in the untreated condition under suitable conditions; soft annealing (+A) is not applicable to boron steels. The Table 7 hardness values do not apply to continuously cast slabs that have not been further deformed. Surface condition at delivery and the type of inspection document are agreed at order.

30MnB5 Heat Treatment

Table 11 of EN 10083-3 gives guidance conditions for heat treating 30MnB5. The austenitizing temperature and quenchant are chosen with the section and shape in mind: the lower end of the hardening range generally applies to water quenching and the upper end to oil quenching. Tempering then sets the final strength level within the Table 8 range.

StepGuidance for 30MnB5
Hardening (austenitizing)860–900 °C
Quenching agentWater
Tempering400–600 °C
End-quench test temperature880 ± 5 °C (mandatory)

Notes: the conditions in Table 11 are for guidance, but the end-quench test temperature is mandatory. Austenitizing time is at least 30 min and tempering time at least 60 min as guide values. When choosing the quenching agent, the shape, dimensions and quenching temperature should be considered because they affect properties and crack susceptibility; synthetic quenchants may also be used.

Related Grades and Alternatives to 30MnB5

Choosing between neighbouring grades is mostly a question of section size and strength class. Compared with 30MnB5: EN 10083-3 20MnB5 steel has lower carbon; EN 10083-3 38MnB5 steel has more carbon; AISI 15B37H boron H-steel is an SAE boron-manganese grade used for similar parts. Similarity listings such as those in GB/T 3077-2015 Annex A are only a comparison aid; chemistry limits and test rules differ, so a substitution should be checked against the governing standard.

Typical Applications of 30MnB5 Plate

Typical uses are wear blades, ground-engaging tools, chains and fasteners made from thin plate or strip and water quenched. In plate form the steel is normally profile-cut, machined and then quenched and tempered, so the purchaser should state whether heat treatment will be done by the mill or by the fabricator, and on what ruling section the properties are to be proven.

30MnB5 Plate Supply and Ordering Information

The supply range below is taken from the original product page and is subject to confirmation for each enquiry.

ItemRange / option
Thickness3 to 300 mm
Width1500 to 4050 mm
Length3000 to 27000 mm
Delivery conditionUntreated or +QT, as agreed
HardenabilityWithout suffix, or +H

Notes: an order should state the standard EN 10083-3, the grade 30MnB5 or number 1.5531, any +H suffix, the delivery condition, the dimensions, whether Table 8 properties are to be tested on a quenched and tempered sample and the inspection document required. Thicknesses above the Table 8 range need agreed property values.

30MnB5 Steel FAQ

What is the chemical composition of EN 10083-3 30MnB5?
Per Table 3, 30MnB5 contains C 0.27–0.33%, Si ≤ 0.40%, Mn 1.15–1.45%, P ≤ 0.025%, S ≤ 0.035% and boron 0.0008–0.0050%. Product analysis may deviate within the Table 4 tolerances.

What are the quenched and tempered properties of 30MnB5 plate?
For t ≤ 8 mm, Table 8 requires Re of at least 800 MPa and Rm of 950–1150 MPa. For the heaviest tabulated plate (8 < t ≤ 20 mm) the values are Re 650 MPa minimum and Rm 800–950 MPa, with elongation of at least 13%.

What heat treatment is recommended for 30MnB5?
Table 11 gives hardening at 860–900 °C, quenching in water, and tempering at 400–600 °C. These are guidance values, but the Jominy test temperature of 880 °C is mandatory.

What does 30MnB5+H mean on an order?
The +H suffix makes the Table 5 Jominy band a requirement. At 1.5 mm from the quenched end the hardness must be 47–56 HRC, and at 15 mm it must be 31–47 HRC.

In which delivery conditions can 30MnB5 plate be ordered?
Untreated is the default, and 30MnB5 is shearable in that condition under suitable conditions (7.3.3). Soft annealing (+A) is not applicable to boron steels. Quenched and tempered (+QT) supply follows Table 8 for the ordered thickness.

Is 30MnB5 shearable without annealing?
Yes. Clause 7.3.3 lists 30MnB5 as shearable in the untreated condition under suitable conditions; soft annealing (+A) is not applicable to boron steels.

Which Chinese grade is similar to 30MnB5?
GB/T 3077-2015 Annex A lists 35MnB as the similar Chinese grade. Check chemistry differences before substituting.