NV A steel plate, also written as DNV Grade A, DNV A, VL A (newer DNV Rules designation) or NV Grade A ship steel plate, is the ordinary-strength hull structural steel of DNV Rules for Classification of Ships (IACS UR W11 ordinary-strength family) with 235 MPa minimum yield, 400-520 MPa tensile strength and Charpy V-notch toughness at +20°C [68°F]. Gangsteel, a steel plate exporter, supplies DNV NV A / Grade A plates cut to size for shipbuilding, offshore platforms and marine structures.
Data source: Per IACS UR W11 (ordinary/higher-strength hull structural steel) as adopted in DNV hull structural steel rules. Official mill/certificate grade is NV A (VL A under current DNV Rules). Verify the current DNV edition before ordering.
| Element | Heat analysis |
|---|---|
| C | 0.21 max |
| Mn | ≥ 2.5×C |
| Si | 0.50 max |
| P | 0.035 max |
| S | 0.035 max |
| C + Mn/6 | 0.40 max (heat) |
Per IACS UR W11 / DNV hull structural steel rules (ordinary-strength grades). Grade A uses a manganese minimum tied to carbon (Mn ≥ 2.5×C) and a C + Mn/6 limit of 0.40%. Grades D and E require fine-grain practice with acid-soluble Al not less than 0.015% when used as the grain-refining element.
When product analysis is required, the finished plate shall meet the heat limits subject to ASTM A6/A6M Table A permitted variations (same practice as other IACS societies), unless a limit is min-only or calculated.
| Element | Heat analysis limit | Product analysis (heat ± A6) |
|---|---|---|
| C | 0.21 max | 0.25 max |
| Mn | ≥ 2.5×C | min-only; product band not tabulated from A6 upper-limit rules |
| Si | 0.50 max | 0.56 max |
| P | 0.035 max | 0.045 max |
| S | 0.035 max | 0.045 max |
| C + Mn/6 | 0.40 max (heat) | calculated from heat analysis |
Per IACS UR W11 / DNV hull structural steel rules. Product analysis applies only when specified.
| Grade | Yield strength, min | Tensile strength | Elongation, min |
|---|---|---|---|
| NV A | 235 MPa [34 ksi] | 400-520 MPa [58-75 ksi] | 22% |
Per IACS UR W11 / DNV hull structural steel rules. Yield and tensile values apply for the full thickness range covered by the grade (typically up to 100 mm for these ship plates).
| Thickness | Test temperature | Longitudinal, avg min | Transverse, avg min |
|---|---|---|---|
| t≤50 mm | +20°C [68°F] | — | — |
| 50<t≤70 mm | +20°C [68°F] | 34 J | 24 J |
| 70<t≤100 mm | +20°C [68°F] | 41 J | 27 J |
Per IACS UR W11 / DNV hull structural steel rules. Average of three full-size Charpy V-notch specimens when impact testing is required; not more than one value below the average and none below 70% of it. For Grade A, impact testing is typically required only above 50 mm. Thicker plates (above 100 mm) may be supplied by agreement with adjusted impact requirements.
Grade A may be as-rolled for thinner plates; thicker plates are often controlled rolled, normalized or TMCP. Deoxidation: any method for Grade A (killed preferred in practice). Optional extras by agreement include ultrasonic testing, Z-direction (Z15/Z25/Z35) through-thickness testing and third-party DNV survey.
Ordinary-strength DNV NV A/B/D/E plates are commonly supplied from about 6 mm to 100 mm thick (up to 150 mm by agreement). Width 1500-4000 mm and length 6000-18000 mm are typical.
| Society / Standard | Equivalent grade |
|---|---|
| DNV | NV A / VL A |
| ABS | ABS Grade A steel plate |
| CCS | CCS Grade A steel plate |
| GL | GL Grade A steel plate |
| BV | BV Grade A steel plate |
| NK | NK Grade A steel plate |
| KR | KR Grade A steel plate |
IACS member societies harmonize ordinary-strength hull grades under UR W11; dual certification is common when ordered that way.
It is an ordinary-strength hull structural steel under DNV Rules for Classification of Ships (IACS UR W11), with 235 MPa minimum yield, 400-520 MPa tensile strength and Charpy toughness requirements at +20°C [68°F] (by thickness).
NV (or VL) is the DNV grade prefix. Grade A is the ordinary-strength toughness class tested at +20°C [68°F] (impact may be waived for Grade A at t≤50 mm per UR W11).
Minimum 235 MPa (34 ksi), tensile 400-520 MPa (58-75 ksi), elongation about 22% min.
Charpy V-notch at +20°C [68°F]. See the impact table for longitudinal/transverse minima by thickness band.
Same 235 MPa ordinary-strength class. Toughness class differs: A at +20°C (often waived ≤50 mm), B at 0°C, D at -20°C, E at -40°C.
Grade A is ordinary strength (235 MPa). NV A32/A36/A40 families are higher-strength (315/355/390 MPa) under the same UR W11 framework.
Yes. Ordinary-strength ship plates are widely welded with standard procedures; follow approved WPS for thickness and Ceq.
Grade A may be as-rolled for thinner plates; thicker plates are often controlled rolled, normalized or TMCP. Deoxidation: any method for Grade A (killed preferred in practice).
Typical supply is about 6-100 mm thick (up to 150 mm by agreement), 1500-4000 mm wide and 6000-18000 mm long.
DNV Grade B steel plate | DNV Grade D steel plate | DNV Grade E steel plate | DNV A32 steel plate | DNV A36 steel plate | DNV A40 steel plate | DNV D32 steel plate | DNV D36 steel plate | DNV D40 steel plate | DNV E32 steel plate | DNV E36 steel plate | DNV E40 steel plate | DNV F32 steel plate | DNV F36 steel plate | DNV F40 steel plate | DNV AH36 steel plate | DNV EH40 steel plate
DNV NV A / Grade A corresponds to the same ordinary-strength grade under other IACS member classification societies: ABS Grade A steel plate, CCS Grade A steel plate, GL Grade A steel plate, BV Grade A steel plate, NK Grade A steel plate, KR Grade A steel plate.
AH36,NV A36|DNV Grade AH36,DNV AH36 STEEL PLATE Gangsteelis specialized in supplying DNVhigh strength steel pla
Grade B,NV B |DNV Grade B,Grade B STEEL PLATE Gangsteel is specialized in supplying DNV general strength steel
Gangsteel is specialized in supplying DNV high strength steel plate in DNV Grade FH36,DNV FH36,NV F36 steel pla
EH36,NV E36|DNV Grade EH36,DNV EH36 STEEL PLATE Gangsteel is specialized in supplying DNV high strength steel p