DNV Steel Plate
DNV E36 Steel Plate | NV E36/EH36 Shipbuilding Plate
NV E36 steel plate, also written as DNV E36, DNV Grade E36, VL E36 (newer DNV Rules designation), EH36 or DNV EH36 ship steel plate, is the higher-strength hull structural steel of DNV Rules for Classification of Ships (IACS UR W11 higher-strength family) with 355 MPa minimum yield, 490-620 MPa tensile strength and Charpy V-notch toughness at -40°C [-40°F]. In the grade name, "E" is the toughness class, and "36" refers to the strength level (historically about 36 kgf/mm²); the market name EH36 adds "H" for higher strength. Gangsteel, a steel plate exporter, supplies DNV NV E36 / EH36 plates cut to size for shipbuilding, offshore platforms and marine structures.
Data source: Per IACS UR W11 (ordinary/higher-strength hull structural steel) as adopted in DNV hull structural steel rules. Official mill/certificate grade is NV E36 (VL E36 under current DNV Rules); EH36 is the common IACS market name. Verify the current DNV edition before ordering.
NV E36 / EH36 Chemical Composition (Heat Analysis)
| Element | C | Mn | Si | P | S | Al (acid sol.) |
|---|---|---|---|---|---|---|
| NV E36 / EH36, % | 0.18 max | 0.90-1.60 | 0.10-0.50 | 0.035 max | 0.035 max | 0.015 min |
| Element | Nb | V | Ti | Cu | Cr | Ni / Mo |
| NV E36 / EH36, % | 0.02-0.05 | 0.05-0.10 | 0.02 max | 0.35 max | 0.20 max | 0.40 max / 0.08 max |
Per IACS UR W11 / DNV hull structural steel rules (higher-strength grades). Nb, V and Al grain-refining elements may be used singly or in combination; when used in combination the individual minima do not apply. Where acid-soluble Al is not less than 0.015%, the Si minimum does not apply. Carbon equivalent: Ceq = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15 (%).
Product Analysis (Check Analysis)
IACS UR W11 / DNV rules do not separately tabulate product (check) analysis limits for higher-strength grades. When product analysis is required, the finished plate shall meet the heat limits subject to ASTM A6/A6M Table A permitted variations (same practice as other IACS societies).
| Element | Heat analysis limit | Product analysis (heat ± A6) |
|---|---|---|
| C | 0.18 max | 0.22 max |
| Mn | 0.90-1.60 | 0.81–1.72 |
| Si | 0.10-0.50 | 0.04–0.56 |
| P | 0.035 max | 0.045 max |
| S | 0.035 max | 0.045 max |
| Al (acid sol.) | 0.015 min | no A6 Table A tolerance; product value not tabulated |
| Nb | 0.02-0.05 | 0.010–0.060 |
| V | 0.05-0.10 | 0.040–0.110 |
| Ti | 0.02 max | 0.03 max |
| Cu | 0.35 max | 0.38 max |
| Cr | 0.20 max | 0.24 max |
| Ni | 0.40 max | 0.43 max |
| Mo | 0.08 max | 0.09 max |
Per IACS UR W11 / DNV hull structural steel rules. Product analysis applies only when specified; for a range, results may not vary both above and below it.
NV E36 Mechanical Properties
| Grade | Yield strength, min | Tensile strength | Elongation, min |
|---|---|---|---|
| NV E36 | 355 MPa [51 ksi] | 490-620 MPa [71-90 ksi] | 21% |
Per IACS UR W11 / DNV hull structural steel rules. Yield and tensile values apply for the full thickness range covered by the grade (typically up to 100 mm for these ship plates).
Charpy V-Notch Impact Requirements (-40°C [-40°F])
| Thickness | Test temperature | Longitudinal, avg min | Transverse, avg min |
|---|---|---|---|
| t≤50 mm | -40°C [-40°F] | 34 J | 24 J |
| 50<t≤70 mm | -40°C [-40°F] | 41 J | 27 J |
| 70<t≤100 mm | -40°C [-40°F] | 50 J | 34 J |
Per IACS UR W11 / DNV hull structural steel rules. Average of three full-size Charpy V-notch specimens; not more than one value below the average and none below 70% of it. Longitudinal values shown; transverse values apply when required by the rules or purchase order. Thicker plates (above 100 mm) may be supplied by agreement with adjusted impact requirements.
Delivery Condition and Deoxidation
Deoxidation: Killed, fine-grain practice. Delivery condition: E-class (NV E36 / EH36) grades are supplied normalized or TMCP; as-rolled delivery is not permitted for the E toughness class. Optional extras by agreement include ultrasonic testing, Z-direction (Z15/Z25/Z35) through-thickness testing and third-party DNV survey.
Thickness Coverage
Higher-strength DNV NV A/D/E/F 32/36/40 plates are commonly supplied from about 6 mm to 100 mm thick (up to 150 mm by agreement). Width 1500-4000 mm and length 6000-18000 mm are typical.
Equivalent Steel Grades of NV E36
| Society / Standard | Equivalent grade |
|---|---|
| DNV | NV E36 / VL E36 (EH36) |
| LR (Lloyd's Register) | LR EH36 steel plate |
| ABS | ABS EH36 steel plate |
| CCS | CCS EH36 steel plate |
| ASTM A131/A131M | ASTM A131 EH36 steel plate |
| GL | GL EH36 steel plate |
| BV | BV EH36 steel plate |
| NK | NK E36 steel plate |
| KR | KR E36 steel plate |
| RINA | RINA EH36 steel plate |
IACS member societies harmonize ordinary and higher-strength hull grades under UR W11; dual certification (for example DNV + ABS, or DNV + ASTM A131) is common when ordered that way.
FAQ about DNV E36 / NV E36 Steel Plate
What is DNV E36 (NV E36) steel plate?
It is a higher-strength hull structural steel under DNV Rules for Classification of Ships (IACS UR W11), with 355 MPa minimum yield, 490-620 MPa tensile strength and Charpy toughness at -40°C [-40°F]. The mill certificate grade is NV E36 (VL E36 in newer DNV Rules); EH36 is the common market name.
What does NV E36 / EH36 stand for?
NV (or VL) is the DNV grade prefix. The letter E is the toughness class (Charpy at -40°C [-40°F]), and 36 is the strength level (historically about 36 kgf/mm², now 355 MPa min yield). EH36 adds "H" for higher strength in the IACS market naming.
What is the yield strength of DNV NV E36?
Minimum 355 MPa (51 ksi), tensile 490-620 MPa (71-90 ksi), elongation about 21% min.
What is the impact test temperature for NV E36?
Charpy V-notch at -40°C [-40°F]. Longitudinal average minima are 34 J up to 50 mm, 41 J for 50-70 mm and 50 J for 70-100 mm.
What is the difference between NV E36 and other 36-class grades?
Same 355 MPa strength class. NV A36 at 0°C [32°F]; NV D36 at -20°C [-4°F]; NV E36 at -40°C [-40°F]; NV F36 at -60°C [-76°F]. Delivery condition follows the toughness letter rules.
What is the difference between NV E36 and NV E32?
Same E-class toughness (Charpy at -40°C [-40°F]). NV E36 is strength class 36 (355 MPa min yield); NV E32 is strength class 32 (315 MPa min yield).
Is NV E36 the same as ABS EH36 or LR EH36?
Requirements are essentially harmonized under IACS UR W11. ABS EH36, LR EH36 and ASTM A131 EH36 (where listed) are counterparts; dual certification is common when ordered with the required surveys.
Is DNV NV E36 weldable?
Yes. Controlled carbon and Ceq give good weldability; preheat may be required for thick sections depending on Ceq and restraint.
What heat treatment is required for NV E36?
E-class (NV E36 / EH36) grades are supplied normalized or TMCP; as-rolled delivery is not permitted for the E toughness class.
What thickness is available for DNV E36?
Typical supply is about 6-100 mm thick (up to 150 mm by agreement), 1500-4000 mm wide and 6000-18000 mm long.
Other DNV Steel Plate Grades
DNV Grade A steel plate | DNV Grade B steel plate | DNV Grade D steel plate | DNV Grade E steel plate | DNV A32 steel plate | DNV A36 steel plate | DNV A40 steel plate | DNV D32 steel plate | DNV D36 steel plate | DNV D40 steel plate | DNV E32 steel plate | DNV E40 steel plate | DNV F32 steel plate | DNV F36 steel plate | DNV F40 steel plate | DNV AH36 steel plate | DNV EH40 steel plate
Equivalent Class Society Grades
DNV NV E36 / EH36 corresponds to the same grade under the other IACS member classification societies and ASTM A131: LR EH36 steel plate, ABS EH36 steel plate, CCS EH36 steel plate, ASTM A131 EH36 steel plate, GL EH36 steel plate, BV EH36 steel plate, NK E36 steel plate, KR E36 steel plate, RINA EH36 steel plate.
-
DNV F36 Steel Plate | NV F36/FH
Gangsteel is specialized in supplying DNV high strength steel plate in DNV Grade FH36,DNV FH36,NV F36 steel pla
-
DNV E36 Steel Plate | NV E36/EH
EH36,NV E36|DNV Grade EH36,DNV EH36 STEEL PLATE Gangsteel is specialized in supplying DNV high strength steel p
-
DNV D36 Steel Plate | NV D36/DH
DH36,NV D36|DNV Grade DH36,DNV DH36 STEEL PLATE Gangsteel is specialized in supplying DNV high strength steel p
-
DNV Grade B Steel Plate | NV B
Grade B,NV B |DNV Grade B,Grade B STEEL PLATE Gangsteel is specialized in supplying DNV general strength steel