High Quality Steel Plate
EN 10028 3 P460NH STEEL Steel Plate Applications & Ordering G
EN 10028-3 P460NH (1.8935) is specified for industrial fabrications where the drawing or material list names this grade. This applications page explains where the grade is used, what service conditions drive selection, and which certificate details belong on the purchase order. Gangsteel supplies EN 10028-3 P460NH (1.8935) with EN 10204 mill test certificates.
This page is a standalone technical article. For the primary overview on the original URL, see EN 10028-3 P460NH (1.8935) primary specification page.
Typical Applications and Service Conditions
EN 10028-3 P460NH (1.8935) plate is ordered for pressure equipment, process vessels, heat-exchanger related fabrications, structural members under the governing code, and project packages that call the grade by name. Match the mill test certificate grade mark to the calculation sheet; do not treat near-equivalents as automatic substitutes.
Service drivers include the design temperature and pressure of the governing code (ASME, EN/PED, class society, or project specification), weld procedure qualification needs, toughness or creep allowables where applicable, and inspection scope. Delivery condition Normalized (+N) should be stated explicitly on the purchase order.
Industry Use Cases
Pressure equipment and process: shells, heads, and related platework when drawings name EN 10028-3 P460NH (1.8935). Power and energy: boiler and heat-recovery fabrications under the ordered edition. Marine / offshore (when classed): only when the society material list names this exact grade stamp. Always keep heat-number traceability on cut pieces.
Chemical Composition - Supporting Data (EN 10028-3 P460NH (1.8935))
Ladle / cast analysis limits. Product analysis tolerances apply per EN 10028-3.
| Element / rule | Requirement |
|---|---|
| C, max | 0.20 |
| Si, max | 0.60 |
| Mn | 1.10-1.70 |
| P, max | 0.025 |
| S, max | 0.010 |
| Al total, min | 0.020 |
| N, max | 0.025 |
| Cr, max | 0.30 |
| Cu, max | 0.70 |
| Mo, max | 0.10 |
| Nb, max | 0.05 |
| Ni, max | 0.80 |
| Ti, max | 0.03 |
| V, max | 0.20 |
| Nb+Ti+V, max | 0.22 |
Mechanical Properties - Supporting Data (EN 10028-3 P460NH (1.8935))
Normalized (+N), transverse. Elongation minimum 16% all listed bands.
| Thickness t (mm) | ReH min (MPa) | Rm (MPa) | A min % |
|---|---|---|---|
| <=16 | 460 | 570-730 | 16 |
| 16 < t <= 40 | 445 | 570-720 | 16 |
| 40 < t <= 60 | 430 | 570-720 | 16 |
| 60 < t <= 100 | 400 | 540-710 | 16 |
| 100 < t <= 150 | 380 | 520-690 | 16 |
| 150 < t <= 250 | 370 | 510-690 | 16 |
Related / Near-Equivalent Grades
Near-equivalents are for cross-reference only. They are not automatic code substitutes. Substitution requires engineer approval and matching certificate scope.
| System | Grade | Note |
|---|---|---|
| EN 10028-3 | P460NL1 / P460NL2 | Same strength family, lower impact temperatures |
| EN 10028-3 | P355NH | Lower yield class |
| ASTM | A537 Class 1 / A516 (approx.) | Not identical - verify code calculation |
| Steel number | 1.8935 | EN designation |
Frequently Asked Questions
Where is EN 10028-3 P460NH (1.8935) typically applied?
EN 10028-3 P460NH (1.8935) is applied where design documents, class material lists, or purchaser specs name this grade for pressure, process, structural, or marine fabrications as applicable. Match the MTC marking to the drawing. Primary overview: EN 10028-3 P460NH (1.8935).
What service conditions drive selection of EN 10028-3 P460NH (1.8935)?
Design temperature and pressure, toughness or creep allowables, weldability, corrosion or process media, and the governing code edition drive selection. Delivery condition Normalized (+N) must align with the ordered specification.
Can a near-equivalent replace EN 10028-3 P460NH (1.8935) on an applications drawing?
Not without redesign and written approval. Near-equivalents differ in chemistry, heat treatment, impact temperature, or product form. Commercial swaps create non-conformance when the dossier names EN 10028-3 P460NH (1.8935).
What fabrication notes matter for EN 10028-3 P460NH (1.8935)?
Use approved WPS/PQR packages for the thickness and filler, control heat input, and preserve heat-number traceability on cut pieces. State any supplementary UT, PMI, or impact tests on the purchase order.
What certificate and marking should an applications PO demand?
EN 10204 3.1 is standard; 3.2 when a purchaser-appointed inspector witnesses tests. The MTC should show heat analysis, tensile results, delivery condition, and heat number aligned with EN 10028-3 P460NH (1.8935).
How should I RFQ EN 10028-3 P460NH (1.8935) plate from Gangsteel for a project?
Send EN 10028-3 P460NH (1.8935), thickness x width x length (or nesting list), quantity, delivery condition, optional NDT/PMI, certificate type, destination, and any dual-mark needs. Note the end use when special flatness or cut-to-size packaging is required.
Ordering and Mill Certificates
State grade EN 10028-3 P460NH (1.8935), dimensions, quantity, delivery condition, optional NDT/PMI, and certificate (EN 10204 3.1 standard; 3.2 when third-party inspection is ordered). Gangsteel supplies export plate and related products with mill test certificates. Contact Gangsteel for stock and mill production RFQs.
-
What Difference of SA 516 Gr 70
ASME SA 516 Gr 70 and SA 516 Gr 70N are both carbon steel plates specified under ASME Section II (equivalent to