ASTM A1011 Sheet & Strip
ASTM A1011 UHSS Grade 100 Type 1 Ultra High Strength Hot Roll

ASTM A1011 UHSS Grade 90 Type 2 — also written ASTM A1011 UHSS Grade 90 Type 2, A1011M UHSS Grade 90 [620] Type 2, A1011 ultra-high strength steel Grade 90 Type 2, SA-1011 UHSS 90 Type 2 — is an ultra-high strength steel designation of ASTM A1011/A1011M for hot-rolled sheet and strip with a minimum yield strength of 90 ksi [620 MPa] and a minimum tensile strength of 100 ksi [690 MPa]. Gangsteel supplies UHSS Grade 90 Type 2 in coils, slit strip and cut-to-length sheets for weight-critical structures.
What is ASTM A1011 UHSS Grade 90 Type 2?
UHSS is the strongest family in A1011, with Grades 90 and 100. Each grade has two types: Type 1 (the default) is a lean microalloyed composition, while Type 2 allows more copper, nickel and chromium (Cu 0.60%, Ni 0.50%, Cr 0.30% max) to support strength in thicker gauges or atmospheric corrosion resistance. UHSS Grade 90 Type 2 is the Type 2 (higher Cu-Ni-Cr) version.
ASTM A1011 UHSS Grade 90 Type 2 Chemical Composition (Heat Analysis, %)
| Designation | C | Mn | P | S | Cu | Ni | Cr | Mo | V | Cb (Nb) | Ti | N |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| UHSS Grade 90 Type 2 | 0.15 | 2.00 | 0.020 | 0.025 | 0.60 | 0.50 | 0.30 | 0.40 | 0.005 min | 0.005 min | 0.005 min | report |
Columbium (niobium), vanadium, titanium or molybdenum are used singly or in combination, with the 0.005% minimum applying only to the elements selected; the purchaser may restrict nitrogen. Aluminium and silicon are reported. Product (check) analysis tolerances follow ASTM A568/A568M.
ASTM A1011 UHSS Grade 90 Type 2 Mechanical Properties
| Property | Requirement |
|---|---|
| Yield strength | 90 ksi [620 MPa] min |
| Tensile strength | 100 ksi [690 MPa] min |
| Elongation in 2 in [50 mm], over 0.097 in [2.5 mm] | ≥16% |
| Elongation in 2 in [50 mm], 0.097 in [2.5 mm] and under | ≥14% |
| Suggested min. inside radius, 90° cold bend | 2½t |
The mechanical requirements are the same for Type 1 and Type 2; the types differ only in chemistry. Tension tests are longitudinal, full thickness, two per heat or 50 tons, with yield by 0.2% offset or 0.5% extension under load.
Delivery Condition and Heat Treatment
ASTM A1011 UHSS Grade 90 Type 2 is delivered in the hot-rolled condition. A1011 does not call for normalizing, quenching or any other post-rolling heat treatment: the strength and ductility are set on the hot strip mill by the chemistry, the finishing temperature, run-out-table cooling and the coiling temperature. The default surface is as rolled with its mill scale, and the purchaser may order the coil pickled (and oiled) or blast cleaned instead. Edges are supplied as mill edge unless cut edge is ordered, and general requirements such as dimensional tolerances, flatness and coil packaging follow ASTM A568/A568M for sheet or ASTM A749/A749M for strip.
| Item | Delivery condition per ASTM A1011/A1011M |
|---|---|
| Condition | Hot rolled (as rolled), coils or cut lengths |
| Surface finish | As rolled with mill scale (default); pickled, or blast cleaned when ordered |
| Oiling | As-rolled material is shipped dry; pickled or blast-cleaned material is oiled unless ordered dry |
| Edges | Mill edge or cut (slit / trimmed) edge |
| Product forms | Sheet (coils, cut-to-length sheets) and strip (narrow coils, slit strip) |
| General requirements | ASTM A568/A568M for sheet; ASTM A749/A749M for strip |
| Heat treatment | None required by A1011; properties come from hot rolling and controlled coiling |
UHSS strip gets its strength from thermomechanical rolling and accelerated cooling. It must not be normalized or hot formed, and welding heat input should be limited to keep the heat-affected zone strength.
Ordering Information
| Ordering item | What to state on the enquiry |
|---|---|
| Standard | ASTM A1011 or A1011M with year of issue (we work to the current edition unless a year is stated) |
| Designation | UHSS Grade 90 Type 2 (Type 1 is assumed if no type is given), e.g. “ASTM A1011M-23, UHSS Grade 620 Type 2, pickled and oiled, 5.0 x 1500 mm coil” |
| Copper bearing | State when copper-bearing steel is required (Cu 0.20% min) |
| Finish | As rolled, pickled, or blast cleaned |
| Oiling | Oiled or dry (pickled / blasted material is normally oiled) |
| Edge | Mill edge or cut edge |
| Dimensions | Thickness, width, and length for cut lengths; coil ID, maximum OD and maximum coil mass for coils |
| Application | Part name or end use, so forming and surface requirements can be checked |
| Reports | Heat analysis and mechanical test report requirements, third-party inspection if any |
Comparable Grades
Approximate counterparts by yield strength (comparison only): EN 10149-2 S600MC, S650MC.
Applications
UHSS Grade 90 Type 2 is used for crane booms and outriggers, truck and trailer frames, lifting equipment, agricultural and forestry machinery and safety-related automotive members where maximum strength-to-weight is needed.
Documents, Inspection and Lead Time
Every ASTM A1011 UHSS Grade 90 Type 2 shipment from Gangsteel is supplied with a mill test certificate to EN 10204 type 3.1 that states the ASTM designation and year, the designation, grade, type or class, the heat number, the heat analysis and, for structural and high-strength designations, the tension test results, together with the purchase order number. Third-party inspection to EN 10204 type 3.2 by SGS, BV, TUV, LR or another agency nominated by the buyer can be arranged before shipment. Each coil or lift carries a tag with the specification, designation, heat number, size and mass.
Lead time is confirmed with each enquiry against the current hot strip mill rolling schedule, the thickness and width mix and any pickling, slitting or cut-to-length processing required, so please send the size list and quantity per item for a firm delivery date.
FAQ
What is the difference between UHSS Grade 90 Type 2 and Type 1?
The strength, elongation and bend requirements are identical. Type 1 limits copper to 0.20%, nickel to 0.20% and chromium to 0.15%; Type 2 allows copper 0.60%, nickel 0.50% and chromium 0.30%. Type 2 gives the producer more alloy freedom, and the copper-nickel-chromium level also improves atmospheric corrosion resistance. Molybdenum is 0.40% max in both.
Can UHSS Grade 90 Type 2 be cold formed?
Yes, within limits. A1011 suggests a minimum inside radius of 2½t for 90° bends in UHSS. Springback is much higher than in mild steel, so tooling must allow for overbending. Edges should be sheared or laser cut cleanly, because burrs and shear cracks start bend cracks at this strength level.
Is UHSS Grade 90 Type 2 weldable?
Yes, with carbon at 0.15% max. Use matching or slightly undermatching low-hydrogen consumables, keep heat input low (multi-pass rather than wide weave) and avoid preheat beyond what the thickness requires, since excess heat softens the heat-affected zone of thermomechanically rolled steel.
What elongation should I expect?
The minimum in 2 in [50 mm] is 16% for thickness over 0.097 in [2.5 mm] and 14% for 0.097 in and under. Actual coils usually exceed these minimums; the real values are reported on the mill certificate.
Which type is supplied if I do not specify it?
A1011 makes Type 1 the default for UHSS. If you need Type 2 chemistry, for example because your design relies on the higher copper level, state it on the order.
Related ASTM A1011 Designations
UHSS Grade 90 Type 1 | UHSS Grade 100 Type 1 | UHSS Grade 100 Type 2 | ASTM A1011/A1011M standard overview