GB/T 1591 Q420MD steel plate

Q420MD — also written GB/T 1591 Q420MD, GB/T 1591-2018 Q420MD, Q420MD steel plate, Q420 M D, Q420MD (TMCP) low alloy high strength steel — is a high-strength low-alloy structural steel of the Chinese standard GB/T 1591-2018, delivered in the thermomechanically rolled (TMCP) condition with a minimum upper yield strength of 420 MPa for thickness up to 16 mm and quality grade D impact toughness. Gangsteel supplies Q420MD steel plate, wide plate and, on request, sections and strip for welded structures in China and export projects.

What is Q420MD?

The designation is built from Q (yield), the minimum upper yield strength 420 MPa, the delivery code M and the quality grade D. GB/T 1591-2018 introduced the delivery code: hot-rolled grades carry no code (for example Q355B), normalized and normalized-rolled grades carry N, and thermomechanically rolled grades carry M. The quality grade sets the impact test temperature: B at 20 °C, C at 0 °C, D at −20 °C, E at −40 °C and F at −60 °C. TMCP steel is rolled with controlled temperature and reduction in the final passes, often followed by accelerated cooling, so the strength comes from a very fine grain at low carbon. This gives lower carbon equivalent and better weldability than a normalized steel of the same strength, but the properties are not retained after normalizing or hot forming. Under the 2008 edition this steel was ordered as Q420D with the delivery condition stated separately.

Q420MD Chemical Composition (Heat Analysis, %)

GB/T 1591-2018 Table 5, heat analysis, maximum % unless a range or minimum is shown
Grade C Si Mn P S Nb V Ti Cr Ni Cu Mo N B Als
Q420MD 0.16 0.50 1.70 0.030 0.025 0.01–0.05 0.01–0.12 0.006–0.05 0.30 0.80 0.40 0.20 0.025 – ≥0.015
  • At least one of the grain-refining elements Al, Nb, V and Ti must be present at or above its listed minimum; when Nb, V or Ti is added to the minimum level, the aluminium minimum does not apply. Total aluminium Alt ≥0.020% may replace acid-soluble aluminium Als ≥0.015%.
  • The titanium maximum may be raised to 0.20%.
  • For sections and bars, phosphorus and sulfur limits may each be 0.005% higher.
  • For sections and bars, the carbon maximum may be 0.02% higher.
  • Product (check) analysis tolerances follow GB/T 222; the steel is made in a converter or electric furnace and may be secondary refined.

Q420MD Carbon Equivalent

GB/T 1591-2018 Table 6, TMCP steels, based on heat analysis
Thickness, mm ≤16 >16–40 >40–63 >63–120 >120–150 (bars only) Pcm max, %
CEV max, % 0.43 0.45 0.46 0.47 0.47 0.20

When the carbon content of a TMCP steel is 0.12% or less, the weld cracking parameter Pcm is used instead of CEV; Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B.

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15, calculated from the heat analysis and reported on the mill certificate.

Q420MD Mechanical Properties

Upper yield strength (Rp0.2 may be used when yield is not distinct)
Thickness, mm ≤16 >16–40 >40–63 >63–80 >80–100 >100–120
ReH min, MPa 420 400 390 380 370 365
Tensile strength
Thickness, mm ≤40 >40–63 >63–80 >80–100 >100–120
Rm, MPa 520–680 500–660 480–640 470–630 460–620

Minimum elongation after fracture A: 19% (GB/T 1591-2018 Table 10). For sections and bars the last thickness band extends to 150 mm.

Tensile test pieces are transverse for plate and strip of width 600 mm or more and longitudinal for other products. Where through-thickness (Z-direction) properties are required, the reduction of area is tested to GB/T 5313 and the suffix Z15, Z25 or Z35 is added to the grade, for example Q420MDZ25.

Q420MD Impact Test (Charpy V-notch)

GB/T 1591-2018 Table 11, average of three specimens
Test temperature KV2 min, longitudinal KV2 min, transverse
20 °C 55 J 31 J
0 °C 47 J 27 J
−20 °C 40 J 20 J

The impact test applies from 6 mm thickness (12 mm diameter for bars), using 10 × 10 × 55 mm specimens; for thinner material 7.5 mm or 5 mm sub-size specimens are used, with 75% and 50% of the required values. Longitudinal specimens are used unless transverse testing is agreed. Unless the order states the test temperature, Q420MD is tested at −20 °C. By agreement, grade D may be tested at −30 °C with KV2 ≥27 J longitudinal.

Bend Test

GB/T 1591-2018 Table 12
Thickness a, mm ≤16 >16–100
180° bend, mandrel diameter D 2a 3a

The bend test is made at the purchaser’s request; it can be omitted when the supplier guarantees the result.

Delivery Condition and Heat Treatment

Q420MD is delivered in the thermomechanically rolled condition (M), which includes TMCP plus tempering. The final rolling passes are made in a temperature range where the austenite does not fully recrystallize, often followed by accelerated cooling. The fine grain produced in this way cannot be reproduced by later heat treatment, so the steel must not be normalized or hot formed by the user; stress relieving after welding is possible but the temperature should be agreed and the procedure qualified.

Item Requirement / practice
Delivery condition Thermomechanically rolled (TMCP), or TMCP + tempering
Normalizing / hot forming by user Not permitted; properties would be lost
Cold forming Suitable; bend to Table 12
Post-weld heat treatment Possible at an agreed temperature; qualify the procedure
Thickness range of the table Up to 120 mm
Dimensions GB/T 709 plate/strip; GB/T 706, GB/T 11263 sections; GB/T 702 bars

Ordering Information

Ordering item What to state on the enquiry
Standard GB/T 1591-2018
Grade Q420MD (add Z15/Z25/Z35 if through-thickness properties are required)
Dimensions Thickness, width, length; tolerance class to GB/T 709 (e.g. class B)
Impact test Test temperature if different from the default, and longitudinal or transverse
Optional tests Bend test, ultrasonic testing (e.g. GB/T 2970 level), product analysis, CEV/Pcm limit
Surface As rolled, shot blasted and primed if required
Inspection Mill certificate 3.1 or third-party 3.2

Comparable Grades

Annex A of GB/T 1591-2018 lists ISO 630-3 S420MD and EN 10025-4 S420M as the comparable grades of Q420MD, and Q420D (TMCP) as the corresponding designation in the 2008 edition. The comparison is approximate: thickness bands, impact energies and CEV limits are not identical, so the exact standard must be stated on the order.

Applications

Q420MD is used for weight-sensitive welded structures with high weldability requirements: bridges, high-rise building columns, wind towers, ship and offshore structures, cranes, construction machinery booms and pipelines. Quality grade D is selected where the lowest service temperature or the design code calls for impact toughness at −20 °C.

Documents, Inspection and Lead Time

Q420MD plates from Gangsteel are supplied with a mill test certificate to EN 10204 type 3.1 (GB/T 247 quality certificate) giving heat analysis, CEV, tensile and impact results and the delivery condition. Acceptance is by batch: each batch is of one grade, heat, size and delivery condition and weighs no more than 60 t, with one tensile test, one bend test (if ordered) and three impact specimens per batch. Third-party inspection to EN 10204 3.2 by SGS, BV, TUV, LR, DNV or ABS can be arranged. Lead time is confirmed with each enquiry against the mill rolling schedule, the thickness and the TMCP route, so please send the size list and quantity.

FAQ

What does each part of the designation Q420MD mean?

Q stands for yield strength, 420 is the minimum upper yield strength in MPa for thickness up to 16 mm, M is the delivery condition (thermomechanically rolled (TMCP)) and D is the quality grade, which sets the Charpy impact requirement. The yield requirement decreases with thickness; for example, it is 390 MPa at 40–63 mm.

What is the difference between Q420MD and Q420ND?

Both have the same minimum yield strength and quality grade, but they are made by different routes. The N grade is normalized, has a ferrite-pearlite structure, allows higher carbon (up to 0.20%) and keeps its properties after hot forming or a later normalizing treatment. The M grade is thermomechanically rolled with lower carbon (0.16% max for Q420M), so its CEV is lower and it welds with less preheat, but it must not be normalized or hot formed. Choose N for hot-formed parts and thick normalized sections, and M for highly welded, weight-optimised structures.

At what temperature is Q420MD impact tested?

Unless the order states otherwise, Q420MD is tested at −20 °C, and the minimum average energy there is 40 J longitudinal (20 J transverse) on 10 mm specimens. The standard also lists the values at higher test temperatures, which apply if the purchaser orders a different test temperature.

Is Q420MD weldable?

Yes. GB/T 1591 controls weldability through the carbon equivalent: for Q420MD the CEV maximum is 0.43 for the thinnest band (up to 16 mm), and Pcm 0.20 maximum applies when carbon is 0.12% or less. With these limits the steel can be welded by SMAW, GMAW, FCAW and SAW using matching low-hydrogen consumables; preheat depends on thickness, CEV, joint restraint and hydrogen level and should be set by the welding procedure qualification.

Which thickness can be supplied in Q420MD?

The property tables of GB/T 1591-2018 for Q420M cover thicknesses up to 120 mm. Plate dimensions and tolerances follow GB/T 709. Send us the thickness, width and length you need and we will confirm the mill and delivery route.

Related GB/T 1591 Grades

Q420MB | Q420MC | Q420ME | Q420ND | Q420D (2008 designation) | GB/T 1591-2018 standard overview

Other Products