GB/T 1591 Q420NB Normalized Steel Plate, Q420N B Grade

Q420NB — also written GB/T 1591 Q420NB, GB/T 1591-2018 Q420NB, Q420NB steel plate, Q420 N B, Q420NB (normalized) low alloy high strength steel — is a high-strength low-alloy structural steel of the Chinese standard GB/T 1591-2018, delivered in the normalized or normalized rolled condition with a minimum upper yield strength of 420 MPa for thickness up to 16 mm and quality grade B impact toughness. Gangsteel supplies Q420NB steel plate, wide plate and, on request, sections and strip for welded structures in China and export projects.
What is Q420NB?
The designation is built from Q (yield), the minimum upper yield strength 420 MPa, the delivery code N and the quality grade B. GB/T 1591-2018 introduced the delivery code: hot-rolled grades carry no code (for example Q355B), normalized and normalized-rolled grades carry N, and thermomechanically rolled grades carry M. The quality grade sets the impact test temperature: B at 20 °C, C at 0 °C, D at −20 °C, E at −40 °C and F at −60 °C. In the normalized condition the steel is heated above Ac3 and air cooled (or the final rolling passes are made in the normalizing temperature range), giving a uniform fine-grained ferrite-pearlite structure whose properties survive a later normalizing or hot forming by the user. Under the 2008 edition this steel was ordered as Q420B with the delivery condition stated separately.
Q420NB Chemical Composition (Heat Analysis, %)
| Grade | C | Si | Mn | P | S | Nb | V | Ti | Cr | Ni | Cu | Mo | N | Als |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Q420NB | 0.20 | 0.60 | 1.00–1.70 | 0.035 | 0.035 | 0.01–0.05 | 0.01–0.20 | 0.006–0.05 | 0.30 | 0.80 | 0.40 | 0.10 | 0.015 | ≥0.015 |
- At least one of the grain-refining elements Al, Nb, V and Ti must be present at or above its listed minimum; when Nb, V or Ti is added to the minimum level, the aluminium minimum does not apply. Total aluminium Alt ≥0.020% may replace acid-soluble aluminium Als ≥0.015%.
- The titanium maximum may be raised to 0.20%.
- For sections and bars, phosphorus and sulfur limits may each be 0.005% higher.
- Product (check) analysis tolerances follow GB/T 222; the steel is made in a converter or electric furnace and may be secondary refined.
Q420NB Carbon Equivalent
| Thickness, mm | ≤63 | >63–100 | >100–250 | >250–400 |
|---|---|---|---|---|
| CEV max, % | 0.48 | 0.50 | 0.52 | by agreement |
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15, calculated from the heat analysis and reported on the mill certificate.
Q420NB Mechanical Properties
| Thickness, mm | ≤16 | >16–40 | >40–63 | >63–80 | >80–100 | >100–150 | >150–200 | >200–250 |
|---|---|---|---|---|---|---|---|---|
| ReH min, MPa | 420 | 400 | 390 | 370 | 360 | 340 | 330 | 320 |
| Thickness, mm | ≤100 | >100–200 | >200–250 |
|---|---|---|---|
| Rm, MPa | 520–680 | 500–650 | 500–650 |
| Thickness, mm | ≤16 | >16–40 | >40–63 | >63–80 | >80–200 | >200–250 |
|---|---|---|---|---|---|---|
| A min, % | 19 | 19 | 19 | 18 | 18 | 18 |
Tensile test pieces are transverse for plate and strip of width 600 mm or more and longitudinal for other products. Where through-thickness (Z-direction) properties are required, the reduction of area is tested to GB/T 5313 and the suffix Z15, Z25 or Z35 is added to the grade, for example Q420NBZ25.
Q420NB Impact Test (Charpy V-notch)
| Test temperature | KV2 min, longitudinal | KV2 min, transverse |
|---|---|---|
| 20 °C | 34 J | 27 J |
The impact test applies from 6 mm thickness (12 mm diameter for bars), using 10 × 10 × 55 mm specimens; for thinner material 7.5 mm or 5 mm sub-size specimens are used, with 75% and 50% of the required values. Longitudinal specimens are used unless transverse testing is agreed.
Bend Test
| Thickness a, mm | ≤16 | >16–100 |
|---|---|---|
| 180° bend, mandrel diameter D | 2a | 3a |
The bend test is made at the purchaser’s request; it can be omitted when the supplier guarantees the result.
Delivery Condition and Heat Treatment
Q420NB is delivered normalized (N) or normalized rolled; the normalized condition includes normalized plus tempered (N+T). In normalizing, the plate is heated to a temperature above Ac3 and cooled in still air; in normalized rolling, the final deformation is carried out in the same temperature range so that the result is equivalent. Because the properties come from a normalized microstructure, they are restored if the user normalizes the plate again, which makes N steels suitable for hot forming and for stress relieving after welding.
| Item | Requirement / practice |
|---|---|
| Delivery condition | Normalized (N), normalized + tempered, or normalized rolled |
| Hot forming by user | Possible in the normalizing range; properties are restored |
| Post-weld heat treatment | Stress relieving possible; qualify the procedure |
| Thickness range of the table | Up to 250 mm (250–400 mm by agreement) |
| Dimensions | GB/T 709 plate/strip; GB/T 706, GB/T 11263 sections; GB/T 702 bars |
Ordering Information
| Ordering item | What to state on the enquiry |
|---|---|
| Standard | GB/T 1591-2018 |
| Grade | Q420NB (add Z15/Z25/Z35 if through-thickness properties are required) |
| Dimensions | Thickness, width, length; tolerance class to GB/T 709 (e.g. class B) |
| Impact test | Test temperature if different from the default, and longitudinal or transverse |
| Optional tests | Bend test, ultrasonic testing (e.g. GB/T 2970 level), product analysis, CEV/Pcm limit |
| Surface | As rolled, shot blasted and primed if required |
| Inspection | Mill certificate 3.1 or third-party 3.2 |
Comparable Grades
Annex A of GB/T 1591-2018 gives Q420B (normalized condition) in the 2008 edition as the corresponding grade of Q420NB and lists no direct ISO 630 or EN 10025 equivalent. For projects specified to European standards, the nearest strength levels are compared on a case-by-case basis.
Applications
Q420NB is used for pressure-free welded structures that need good toughness after forming: bridges, building frames, cranes, offshore and port equipment, wind tower flanges and transition pieces, mining machinery and storage tanks. Quality grade B is selected where the lowest service temperature or the design code calls for impact toughness at 20 °C.
Documents, Inspection and Lead Time
Q420NB plates from Gangsteel are supplied with a mill test certificate to EN 10204 type 3.1 (GB/T 247 quality certificate) giving heat analysis, CEV, tensile and impact results and the delivery condition. Acceptance is by batch: each batch is of one grade, heat, size and delivery condition and weighs no more than 60 t, with one tensile test, one bend test (if ordered) and three impact specimens per batch. Third-party inspection to EN 10204 3.2 by SGS, BV, TUV, LR, DNV or ABS can be arranged. Lead time is confirmed with each enquiry against the mill rolling schedule, the thickness and the normalizing route, so please send the size list and quantity.
FAQ
What does each part of the designation Q420NB mean?
Q stands for yield strength, 420 is the minimum upper yield strength in MPa for thickness up to 16 mm, N is the delivery condition (normalized or normalized rolled) and B is the quality grade, which sets the Charpy impact requirement. The yield requirement decreases with thickness; for example, it is 390 MPa at 40–63 mm.
What is the difference between Q420NB and Q420MB?
Both have the same minimum yield strength and quality grade, but they are made by different routes. The N grade is normalized, has a ferrite-pearlite structure, allows higher carbon (up to 0.20%) and keeps its properties after hot forming or a later normalizing treatment. The M grade is thermomechanically rolled with lower carbon (0.16% max for Q420M), so its CEV is lower and it welds with less preheat, but it must not be normalized or hot formed. Choose N for hot-formed parts and thick normalized sections, and M for highly welded, weight-optimised structures.
At what temperature is Q420NB impact tested?
Unless the order states otherwise, Q420NB is tested at 20 °C, and the minimum average energy there is 34 J longitudinal (27 J transverse) on 10 mm specimens. The test is made on three specimens per batch, taken from one end of the product.
Is Q420NB weldable?
Yes. GB/T 1591 controls weldability through the carbon equivalent: for Q420NB the CEV maximum is 0.48 for the thinnest band (up to 63 mm). With these limits the steel can be welded by SMAW, GMAW, FCAW and SAW using matching low-hydrogen consumables; preheat depends on thickness, CEV, joint restraint and hydrogen level and should be set by the welding procedure qualification.
Which thickness can be supplied in Q420NB?
The property tables of GB/T 1591-2018 for Q420N cover thicknesses up to 250 mm (up to 400 mm by agreement for the CEV limits). Plate dimensions and tolerances follow GB/T 709. Send us the thickness, width and length you need and we will confirm the mill and delivery route.
Related GB/T 1591 Grades
Q420NC | Q420ND | Q420NE | Q420MB | Q420B (hot rolled) | GB/T 1591-2018 standard overview
-
GB-T1591 Q460D Steel plate supp
Gangsteel sell GB-T1591 Q460D Low alloy and high strength steel plate, heavy plate and wide, heavy plate.
-
GB-T1591 Q345E Steel Plate supp
Gangsteel sell GB-T1591 Q345E Low alloy and high strength steel plate, heavy plate and wide, heavy plate,
-
GB-T1591 Q345D Carbon steel pla
Gangsteel sell GB-T1591 Q345D Low alloy and high strength steel plate, heavy plate and wide, heavy plate, Which
-
GB-T1591 Q345B Carbon steel pla
Gangsteel sell GB-T1591 Q345B Low alloy and high strength steel plate, heavy plate and wide, heavy plate,