EN 10083-3 Alloy Steel Plate

EN10083-3 34CrMo4 STEEL PLATE

Gangsteel (HENAN GANG IRON AND STEEL CO.,LTD.) supplies EN 10083-3 34CrMo4 (steel number 1.7220) as hot-rolled plate for parts that are cut, machined and then quenched and tempered. EN 10083-3:2006 classifies 34CrMo4 as a chromium-molybdenum steel for quenching and tempering: C 0.30–0.37%, Mn 0.60–0.90%, chromium 0.90–1.20%, molybdenum 0.15–0.30%. It is a medium-carbon Cr-Mo grade with a deep +H band and tabulated properties up to the largest ruling section of the standard, which makes it a frequent choice for heavier quenched and tempered parts. This page sets out the chemistry, the quenched and tempered property table, the Jominy hardenability band, delivery conditions and heat treatment guidance from the standard, so that a purchase order can name exactly what is needed.

What is EN 10083-3 34CrMo4?

EN 10083-3 is Part 3 of the European standard for steels for quenching and tempering and covers the alloy grades (Part 2 covers the non-alloy grades). Its scope includes semi-finished products, bars, rod, wide flats, forgings and hot-rolled strip and sheet/plate. All grades are special steels; the standard requires a fine austenite grain size of 5 or finer and a special-steel level of cleanness. 34CrMo4 indicates about 0.34% mean carbon; the suffix 4 refers to chromium (about 1% after dividing by the factor 4), with molybdenum present. The steel number 1.7220 identifies the same grade in the EN 10027-2 numbering system.

The grade can be ordered with or without hardenability requirements. Without a suffix, the order is governed by the chemical composition and the mechanical properties after quenching and tempering. With the suffix +H, the Jominy hardenability band of Table 5 becomes a requirement and, for the restricted bands, +HH or +HL from Table 6 can be ordered. Either way, the steel is designed to be hardened by the user; plate in the as-rolled condition does not yet have the tabulated strength.

34CrMo4 Chemical Composition (EN 10083-3:2006 Table 3)

Table 3 gives the cast analysis. The ranges below are those printed for 34CrMo4 (1.7220); elements not quoted may not be added intentionally without the purchaser’s agreement, except for finishing the heat.

Grade (number)C %Si %Mn %P %S %Cr %Mo %
34CrMo4 (1.7220)0.30–0.37≤ 0.400.60–0.90≤ 0.025≤ 0.0350.90–1.200.15–0.30

Product (check) analysis may deviate from the cast analysis by the amounts in Table 4. For this grade the relevant permissible deviations are:

ElementCast analysis, %Permissible deviation, %
C0.30–0.37±0.02
Si≤ 0.40+0.03
Mn0.60–0.90±0.04
P≤ 0.025+0.005
S≤ 0.035+0.005
Cr0.90–1.20±0.05
Mo0.15–0.30±0.03

Notes: deviations in product analysis apply to individual elements; within one cast, the deviation of an element may lie above the upper limit or below the lower limit of the Table 3 range, but not both at the same time. For improved machinability, the standard allows sulphur up to about 0.10% to be agreed at the time of enquiry and order, in which case the manganese maximum may be raised by 0.15%.

34CrMo4 Mechanical Properties, Quenched and Tempered (+QT, Table 8)

Table 8 gives minimum yield strength, the tensile strength range, elongation, reduction of area and Charpy V-notch energy for 34CrMo4 after quenching and tempering, listed by ruling section. For flat products the ruling section is the thickness t; the round-bar diameter d of the same column is shown for comparison. For 34CrMo4, values are tabulated up to t ≤ 160 mm.

Plate thickness t, mmBar diameter d, mmRe min, MPaRm, MPaA min, %Z min, %KV min, J
t ≤ 8d ≤ 168001000–12001145–
8 < t ≤ 2016 < d ≤ 40650900–1100125040
20 < t ≤ 6040 < d ≤ 100550800–950145545
60 < t ≤ 100100 < d ≤ 160500750–900155545
100 < t ≤ 160160 < d ≤ 250450700–850156045

Notes: Re is the upper yield strength or, where no yield phenomenon occurs, the 0.2% proof strength Rp0.2. Impact values are not specified for the thinnest ruling section. The original page lists plate up to 300 mm thick; Table 8 stops at t ≤ 160 mm for this grade, so for thicker plate the mechanical requirements must be agreed for the actual product at the time of order. Not all flat-product dimensions can be supplied in the +QT condition.

34CrMo4+H Hardenability Band (Jominy, Table 5)

The end-quench (Jominy) test according to EN ISO 642 measures how hardness falls with distance from the water-quenched end of a standard bar. For 34CrMo4+H the test is carried out from 850 °C, and the measured hardness must stay within the band below. The band describes the steel’s capacity to harden; it is the most direct way to check whether a cast will through-harden in a given section.

Distance from quenched end, mmHRC maxHRC min
1.55749
35749
55748
75645
95542
115439
135336
155234
204830
254528
304327
354126
404025
454024
503924

Notes: a dash means no limit is set at that distance. The values apply to the +H grade only; a grade ordered without +H is not tested against the band. Table 6 additionally defines restricted scatter bands, +HH (narrowed toward the upper part of the band) and +HL (narrowed toward the lower part), for this grade when tighter control of hardenability is needed.

34CrMo4 Delivery Condition

Table 1 of EN 10083-3 lists the heat treatment conditions in which products can be delivered. If nothing is agreed, the steel is supplied untreated, i.e. as hot rolled. For plate in 34CrMo4 the usual choices are untreated (for later quenching and tempering by the fabricator), a condition that eases shearing and machining, or quenched and tempered to a Table 8 property class.

ConditionSymbolRequirement for 34CrMo4
Untreatednone or +UDefault when not agreed; as-rolled, for heat treatment by the user
Treated to improve shearability+SMax. HBW: 255
Soft annealed+AMax. HBW: 223
Quenched and tempered+QTTable 8 properties for the ordered thickness
Otherby agreemente.g. annealing to a certain structure, agreed at enquiry and order

Notes: for the untreated, +S and +A conditions the Table 8 properties must still be achievable after correct quenching and tempering. 34CrMo4 is shearable under suitable conditions in the +S condition with the Table 7 hardness, and in the +A condition. The Table 7 hardness values do not apply to continuously cast slabs that have not been further deformed. Surface condition at delivery and the type of inspection document are agreed at order.

34CrMo4 Heat Treatment

Table 11 of EN 10083-3 gives guidance conditions for heat treating 34CrMo4. The austenitizing temperature and quenchant are chosen with the section and shape in mind: the lower end of the hardening range generally applies to water quenching and the upper end to oil quenching. Tempering then sets the final strength level within the Table 8 range.

StepGuidance for 34CrMo4
Hardening (austenitizing)830–890 °C
Quenching agentOil or water
Tempering540–680 °C
End-quench test temperature850 ± 5 °C (mandatory)

Notes: the conditions in Table 11 are for guidance, but the end-quench test temperature is mandatory. Austenitizing time is at least 30 min and tempering time at least 60 min as guide values. When choosing the quenching agent, the shape, dimensions and quenching temperature should be considered because they affect properties and crack susceptibility; synthetic quenchants may also be used.

Related Grades and Alternatives to 34CrMo4

Choosing between neighbouring grades is mostly a question of section size and strength class. Compared with 34CrMo4: EN 10083-3 25CrMo4 steel is the lower-carbon Cr-Mo grade; EN 10083-3 42CrMoS4 steel is the higher-carbon Cr-Mo grade with controlled sulphur; GB/T 3077 35CrMo steel is listed as similar in GB/T 3077-2015 Annex A; AISI 4137 Cr-Mo steel belongs to the ASTM 4130–4135 family that the same annex names. Similarity listings such as those in GB/T 3077-2015 Annex A are only a comparison aid; chemistry limits and test rules differ, so a substitution should be checked against the governing standard.

Typical Applications of 34CrMo4 Plate

Typical uses are shafts, gears, axles, high-strength fasteners and pressure-loaded components, and plate parts machined into flanges or rings before heat treatment. In plate form the steel is normally profile-cut, machined and then quenched and tempered, so the purchaser should state whether heat treatment will be done by the mill or by the fabricator, and on what ruling section the properties are to be proven.

34CrMo4 Plate Supply and Ordering Information

The supply range below is taken from the original product page and is subject to confirmation for each enquiry.

ItemRange / option
Thickness3 to 300 mm
Width1500 to 4050 mm
Length3000 to 27000 mm
Delivery conditionUntreated, +S, +A or +QT, as agreed
HardenabilityWithout suffix, or +H / +HH / +HL

Notes: an order should state the standard EN 10083-3, the grade 34CrMo4 or number 1.7220, any +H suffix, the delivery condition, the dimensions, whether Table 8 properties are to be tested on a quenched and tempered sample and the inspection document required. Thicknesses above the Table 8 range need agreed property values.

34CrMo4 Steel FAQ

What is the chemical composition of EN 10083-3 34CrMo4?
Per Table 3, 34CrMo4 contains C 0.30–0.37%, Si ≤ 0.40%, Mn 0.60–0.90%, P ≤ 0.025%, S ≤ 0.035% and chromium 0.90–1.20%, molybdenum 0.15–0.30%. Product analysis may deviate within the Table 4 tolerances.

What are the quenched and tempered properties of 34CrMo4 plate?
For t ≤ 8 mm, Table 8 requires Re of at least 800 MPa and Rm of 1000–1200 MPa. For the heaviest tabulated plate (100 < t ≤ 160 mm) the values are Re 450 MPa minimum and Rm 700–850 MPa, with elongation of at least 15%.

What heat treatment is recommended for 34CrMo4?
Table 11 gives hardening at 830–890 °C, quenching in oil or water, and tempering at 540–680 °C. These are guidance values, but the Jominy test temperature of 850 °C is mandatory.

What does 34CrMo4+H mean on an order?
The +H suffix makes the Table 5 Jominy band a requirement. At 1.5 mm from the quenched end the hardness must be 49–57 HRC, and at 15 mm it must be 34–52 HRC.

In which delivery conditions can 34CrMo4 plate be ordered?
Untreated is the default. The +S condition has a maximum of 255 HBW. For +A the maximum is 223 HBW. Quenched and tempered (+QT) supply follows Table 8 for the ordered thickness.

Up to what thickness does EN 10083-3 give properties for 34CrMo4 plate?
Table 8 covers flat products up to 160 mm ruling thickness for 34CrMo4, in five ruling-section steps. Thicker plate is outside the tabulated range and needs agreed requirements.

Which Chinese grades are similar to 34CrMo4?
GB/T 3077-2015 Annex A lists 30CrMo and 35CrMo as similar Chinese grades, with ASTM 4130/4135 and JIS SCM430/SCM435. These are comparison references only.