EN 10083-3 Alloy Steel Plate
EN 10083-3 36NiCrMo16 (1.6773) Plate: Chemistry, QT & H-Band
Gangsteel (HENAN GANG IRON AND STEEL CO.,LTD.) supplies EN 10083-3 36NiCrMo16 (steel number 1.6773) as hot-rolled plate for parts that are cut, machined and then quenched and tempered. EN 10083-3:2006 classifies 36NiCrMo16 as a high-nickel chromium-molybdenum steel for quenching and tempering: C 0.32–0.39%, Mn 0.50–0.80%, chromium 1.60–2.00%, molybdenum 0.25–0.45%, nickel 3.6–4.1%. With about 4% nickel together with chromium and molybdenum it has the flattest hardenability band of the standard and keeps high strength and toughness through very large sections; Table 11 even lists air among its quenching agents. This page sets out the chemistry, the quenched and tempered property table, the Jominy hardenability band, delivery conditions and heat treatment guidance from the standard, so that a purchase order can name exactly what is needed.
What is EN 10083-3 36NiCrMo16?
EN 10083-3 is Part 3 of the European standard for steels for quenching and tempering and covers the alloy grades (Part 2 covers the non-alloy grades). Its scope includes semi-finished products, bars, rod, wide flats, forgings and hot-rolled strip and sheet/plate. All grades are special steels; the standard requires a fine austenite grain size of 5 or finer and a special-steel level of cleanness. 36NiCrMo16 indicates about 0.36% mean carbon; the suffix 16 refers to nickel divided by the factor 4, about 4% Ni, consistent with the tabulated 3.6–4.1% Ni, with chromium and molybdenum also present. The steel number 1.6773 identifies the same grade in the EN 10027-2 numbering system.
The grade can be ordered with or without hardenability requirements. Without a suffix, the order is governed by the chemical composition and the mechanical properties after quenching and tempering. With the suffix +H, the Jominy hardenability band of Table 5 becomes a requirement and, for the restricted bands, +HH or +HL from Table 6 can be ordered. Either way, the steel is designed to be hardened by the user; plate in the as-rolled condition does not yet have the tabulated strength.
36NiCrMo16 Chemical Composition (EN 10083-3:2006 Table 3)
Table 3 gives the cast analysis. The ranges below are those printed for 36NiCrMo16 (1.6773); elements not quoted may not be added intentionally without the purchaser’s agreement, except for finishing the heat.
| Grade (number) | C % | Si % | Mn % | P % | S % | Cr % | Mo % | Ni % |
|---|---|---|---|---|---|---|---|---|
| 36NiCrMo16 (1.6773) | 0.32–0.39 | ≤ 0.40 | 0.50–0.80 | ≤ 0.025 | ≤ 0.025 | 1.60–2.00 | 0.25–0.45 | 3.6–4.1 |
Product (check) analysis may deviate from the cast analysis by the amounts in Table 4. For this grade the relevant permissible deviations are:
| Element | Cast analysis, % | Permissible deviation, % |
|---|---|---|
| C | 0.32–0.39 | ±0.02 |
| Si | ≤ 0.40 | +0.03 |
| Mn | 0.50–0.80 | ±0.04 |
| P | ≤ 0.025 | +0.005 |
| S | ≤ 0.025 | +0.005 |
| Cr | 1.60–2.00 | ±0.05 |
| Mo | 0.25–0.45 | ±0.04 |
| Ni | 3.6–4.1 | ±0.07 |
Notes: deviations in product analysis apply to individual elements; within one cast, the deviation of an element may lie above the upper limit or below the lower limit of the Table 3 range, but not both at the same time. For improved machinability, the standard allows sulphur up to about 0.10% to be agreed at the time of enquiry and order, in which case the manganese maximum may be raised by 0.15%.
36NiCrMo16 Mechanical Properties, Quenched and Tempered (+QT, Table 8)
Table 8 gives minimum yield strength, the tensile strength range, elongation, reduction of area and Charpy V-notch energy for 36NiCrMo16 after quenching and tempering, listed by ruling section. For flat products the ruling section is the thickness t; the round-bar diameter d of the same column is shown for comparison. For 36NiCrMo16, values are tabulated up to t ≤ 160 mm.
| Plate thickness t, mm | Bar diameter d, mm | Re min, MPa | Rm, MPa | A min, % | Z min, % | KV min, J |
|---|---|---|---|---|---|---|
| t ≤ 8 | d ≤ 16 | 1050 | 1250–1450 | 9 | 40 | – |
| 8 < t ≤ 20 | 16 < d ≤ 40 | 1050 | 1250–1450 | 9 | 40 | 30 |
| 20 < t ≤ 60 | 40 < d ≤ 100 | 900 | 1100–1300 | 10 | 45 | 35 |
| 60 < t ≤ 100 | 100 < d ≤ 160 | 800 | 1000–1200 | 11 | 50 | 45 |
| 100 < t ≤ 160 | 160 < d ≤ 250 | 800 | 1000–1200 | 11 | 50 | 45 |
Notes: Re is the upper yield strength or, where no yield phenomenon occurs, the 0.2% proof strength Rp0.2. Impact values are not specified for the thinnest ruling section. The original page lists plate up to 300 mm thick; Table 8 stops at t ≤ 160 mm for this grade, so for thicker plate the mechanical requirements must be agreed for the actual product at the time of order. Not all flat-product dimensions can be supplied in the +QT condition.
36NiCrMo16+H Hardenability Band (Jominy, Table 5)
The end-quench (Jominy) test according to EN ISO 642 measures how hardness falls with distance from the water-quenched end of a standard bar. For 36NiCrMo16+H the test is carried out from 850 °C, and the measured hardness must stay within the band below. The band describes the steel’s capacity to harden; it is the most direct way to check whether a cast will through-harden in a given section.
| Distance from quenched end, mm | HRC max | HRC min |
|---|---|---|
| 1.5 | 57 | 50 |
| 3 | 56 | 49 |
| 5 | 56 | 48 |
| 7 | 56 | 48 |
| 9 | 56 | 48 |
| 11 | 56 | 48 |
| 13 | 55 | 47 |
| 15 | 55 | 47 |
| 20 | 55 | 47 |
| 25 | 55 | 47 |
| 30 | 55 | 47 |
| 35 | 55 | 47 |
| 40 | 55 | 47 |
| 45 | 55 | 47 |
| 50 | 55 | 47 |
Notes: a dash means no limit is set at that distance. The values apply to the +H grade only; a grade ordered without +H is not tested against the band. Table 6 additionally defines restricted scatter bands, +HH (narrowed toward the upper part of the band) and +HL (narrowed toward the lower part), for this grade when tighter control of hardenability is needed.
36NiCrMo16 Delivery Condition
Table 1 of EN 10083-3 lists the heat treatment conditions in which products can be delivered. If nothing is agreed, the steel is supplied untreated, i.e. as hot rolled. For plate in 36NiCrMo16 the usual choices are untreated (for later quenching and tempering by the fabricator), a condition that eases shearing and machining, or quenched and tempered to a Table 8 property class.
| Condition | Symbol | Requirement for 36NiCrMo16 |
|---|---|---|
| Untreated | none or +U | Default when not agreed; as-rolled, for heat treatment by the user |
| Treated to improve shearability | +S | No value given; order +A where shearability matters |
| Soft annealed | +A | Max. HBW: 269 |
| Quenched and tempered | +QT | Table 8 properties for the ordered thickness |
| Other | by agreement | e.g. annealing to a certain structure, agreed at enquiry and order |
Notes: for the untreated, +S and +A conditions the Table 8 properties must still be achievable after correct quenching and tempering. No +S value is given for 36NiCrMo16; where shearability is important, the standard recommends ordering it soft annealed (+A). The Table 7 hardness values do not apply to continuously cast slabs that have not been further deformed. Surface condition at delivery and the type of inspection document are agreed at order.
36NiCrMo16 Heat Treatment
Table 11 of EN 10083-3 gives guidance conditions for heat treating 36NiCrMo16. The austenitizing temperature and quenchant are chosen with the section and shape in mind: the lower end of the hardening range generally applies to water quenching and the upper end to oil quenching. Tempering then sets the final strength level within the Table 8 range.
| Step | Guidance for 36NiCrMo16 |
|---|---|
| Hardening (austenitizing) | 865–885 °C |
| Quenching agent | Air, oil or water |
| Tempering | 550–650 °C |
| End-quench test temperature | 850 ± 5 °C (mandatory) |
Notes: the conditions in Table 11 are for guidance, but the end-quench test temperature is mandatory. Austenitizing time is at least 30 min and tempering time at least 60 min as guide values. When choosing the quenching agent, the shape, dimensions and quenching temperature should be considered because they affect properties and crack susceptibility; synthetic quenchants may also be used.
Related Grades and Alternatives to 36NiCrMo16
Choosing between neighbouring grades is mostly a question of section size and strength class. Compared with 36NiCrMo16: EN 10083-3 34CrNiMo6 steel is the leaner Ni-Cr-Mo grade for medium sections; EN 10083-3 39NiCrMo3 steel has much lower nickel and a steeper band; AISI 4340H Ni-Cr-Mo steel is a widely used American Ni-Cr-Mo grade with lower nickel; GB/T 3077-2015 Annex A pairs 36NiCrMo16 with 35Cr2Ni4Mo instead. Similarity listings such as those in GB/T 3077-2015 Annex A are only a comparison aid; chemistry limits and test rules differ, so a substitution should be checked against the governing standard.
Typical Applications of 36NiCrMo16 Plate
Typical uses are heavily stressed large-section parts such as heavy shafts, high-duty gears, tooling and defence or aerospace-type components, where both strength and toughness must be kept in the core. In plate form the steel is normally profile-cut, machined and then quenched and tempered, so the purchaser should state whether heat treatment will be done by the mill or by the fabricator, and on what ruling section the properties are to be proven.
36NiCrMo16 Plate Supply and Ordering Information
The supply range below is taken from the original product page and is subject to confirmation for each enquiry.
| Item | Range / option |
|---|---|
| Thickness | 3 to 300 mm |
| Width | 1500 to 4050 mm |
| Length | 3000 to 27000 mm |
| Delivery condition | Untreated, +A or +QT, as agreed |
| Hardenability | Without suffix, or +H / +HH / +HL |
Notes: an order should state the standard EN 10083-3, the grade 36NiCrMo16 or number 1.6773, any +H suffix, the delivery condition, the dimensions, whether Table 8 properties are to be tested on a quenched and tempered sample and the inspection document required. Thicknesses above the Table 8 range need agreed property values.
36NiCrMo16 Steel FAQ
What is the chemical composition of EN 10083-3 36NiCrMo16?
Per Table 3, 36NiCrMo16 contains C 0.32–0.39%, Si ≤ 0.40%, Mn 0.50–0.80%, P ≤ 0.025%, S ≤ 0.025% and chromium 1.60–2.00%, molybdenum 0.25–0.45%, nickel 3.6–4.1%. Product analysis may deviate within the Table 4 tolerances.
What are the quenched and tempered properties of 36NiCrMo16 plate?
For t ≤ 8 mm, Table 8 requires Re of at least 1050 MPa and Rm of 1250–1450 MPa. For the heaviest tabulated plate (100 < t ≤ 160 mm) the values are Re 800 MPa minimum and Rm 1000–1200 MPa, with elongation of at least 11%.
What heat treatment is recommended for 36NiCrMo16?
Table 11 gives hardening at 865–885 °C, quenching in air, oil or water, and tempering at 550–650 °C. These are guidance values, but the Jominy test temperature of 850 °C is mandatory.
What does 36NiCrMo16+H mean on an order?
The +H suffix makes the Table 5 Jominy band a requirement. At 1.5 mm from the quenched end the hardness must be 50–57 HRC, and at 15 mm it must be 47–55 HRC.
In which delivery conditions can 36NiCrMo16 plate be ordered?
Untreated is the default. No +S value is given for 36NiCrMo16, so where shearability matters it should be ordered soft annealed. For +A the maximum is 269 HBW. Quenched and tempered (+QT) supply follows Table 8 for the ordered thickness.
Can 36NiCrMo16 be air hardened?
Table 11 lists air, oil or water as quenching agents for 36NiCrMo16, reflecting its very high hardenability. Whether air cooling reaches the required properties depends on section size and must be proven on the ordered thickness.
Why is 36NiCrMo16 more expensive than 34CrNiMo6?
It contains about 3.6–4.1% nickel, more than twice the 1.30–1.70% of 34CrNiMo6, together with more chromium and molybdenum. The alloy content buys a flatter hardenability band and properties in larger sections.
-
EN 10083-3 33MnCrB5-2 (1.7185)
EN 10083-3 33MnCrB5-2 plate: C 0.30–0.36%, Cr 0.30–0.60%, B 0.0008–0.0050%; QT Re ≥850 MPa (t ≤8 mm),
-
EN 10083-3 27MnCrB5-2 (1.7182)
EN 10083-3 27MnCrB5-2 plate: C 0.24–0.30%, Cr 0.30–0.60%, B 0.0008–0.0050%; QT Re ≥800 MPa (t ≤8 mm),
-
EN10083-3 30MnB5 STEEL PLATE
EN 10083-3 30MnB5 (1.5531) alloy steel plate: C 0.27–0.33%, B 0.0008–0.0050%, Mn 1.15–1.45%; QT Re ≥800
-
EN10083-3 20MnB5 STEEL PLATE
EN 10083-3 20MnB5 (1.5530) alloy steel plate: C 0.17–0.23%, B 0.0008–0.0050%, Mn 1.10–1.40%; QT Re ≥700