A516 Grade 70 + Alloy C276 clad steel plate bonds a low-carbon nickel-molybdenum-chromium-tungsten alloy (UNS N10276) to a carbon steel pressure backing. Gangsteel supplies it to ASTM A265 for flue-gas desulfurization, pickling and mixed-acid chemical equipment.

A516 Grade 70 + Alloy C276 N10276 Clad Steel Plate - generated product illustration

Material Pair and Engineering Use

C276 combines 15–17% molybdenum, 14.5–16.5% chromium and 3–4.5% tungsten with very low carbon and silicon. That makes it resistant to both oxidizing and reducing media, including wet chlorine and hypochlorite, and to localized corrosion. As cladding it gives that resistance on a carbon steel wall.

Material identity and specification basis
Part Designation Role
Backing ASTM A516/A516M-25 Grade 70 (Grade 60 by order) Carries pressure and structural load
Cladding ASTM B575-17(2023) UNS N10276 Nickel-alloy corrosion face
Clad product ASTM A265 (A265-12(2026) scope; clauses from 12(2019)) Bond, tests and tolerances

Backing Steel Chemical Composition

A516/A516M-25 Grade 70 [485] backing steel: selected heat-analysis requirements, mass %
Backing thickness C max Mn Si P max S max
≤12.5 mm 0.27 0.85–1.20 0.15–0.40 0.025 0.025
>12.5–50 mm 0.28 0.85–1.20 0.15–0.40 0.025 0.025
>50–100 mm 0.30 0.85–1.20 0.15–0.40 0.025 0.025
>100 mm 0.31 0.85–1.20 0.15–0.40 0.025 0.025

The thickness column refers to the steel backing alone. A516/A516M-25 allows 0.06 percentage point more manganese for each 0.01 point of carbon below the maximum, capped at 1.50% (heat) and 1.60% (product). Where Grade 60 backing is ordered instead, its lower carbon maxima and its own 415–550 MPa tensile range apply; the two grades must not be mixed on one certificate.

Cladding Chemical Composition

ASTM B575-17(2023) UNS N10276 cladding chemistry
Element Requirement, mass %
Ni Remainder (by difference)
Mo 15.0–17.0
Cr 14.5–16.5
Fe 4.0–7.0
W 3.0–4.5
Co ≤2.5
C ≤0.010
Si ≤0.08
Mn ≤1.0
V ≤0.35
P ≤0.04
S ≤0.03

The 0.010% carbon and 0.08% silicon maxima are what distinguish C276 from older C-type alloys and limit grain-boundary precipitation in welded and heat-affected zones.

Mechanical Properties of the Layers and the Bond

Constituent room-temperature reference values (separate layers, not a composite guarantee)
Layer / reference Condition Yield / Rp0.2 min, MPa Tensile, MPa Elongation min
A516/A516M-25 Grade 70 [485] backing Plate as ordered; normalized above 1.5 in. [40 mm] 260 485–620 21% in 50 mm; 17% in 200 mm
N10276 facing, B575-17(2023) Solution annealed plate 283 690 min 40%

The facing row is the annealed flat-product reference of its own specification. It is not added to the backing strength, and bond shear is not a substitute for backing tensile strength. Cladding strength counts in design only where the construction code allows it. B575 lists 100 HRB maximum hardness for information only.

Finished-plate acceptance under ASTM A265-12(2019) clauses
Item Requirement or condition Order meaning
Tensile section Grade 70 backing minima (485 MPa tensile, 260 MPa yield) fall within the 70 ksi / 40 ksi limits; total gage then decides Up to 1.5 in. (about 38 mm) total gage, test the composite section unless the facing is declared corrosion allowance only; above that gage, test the backing alone.
Composite tensile ceiling Up to 5 ksi (35 MPa) above the backing maximum Applies only to the composite-section route; it is not a design strength.
Interface shear (when specified) 20 ksi (140 MPa) minimum Bond property only. Below or at 0.075 in. (1.9 mm) facing, shear testing needs agreement; three bond bend tests are the alternative route.
Bond area Ultrasonic method, coverage and acceptance class agreed on the order One shear coupon does not show that the whole C276 face is bonded.

Inch-pound values govern in the ASTM clad specifications; metric figures are conversions. The scope of A265 is confirmed against the A265-12(2026) listing, while the clause wording above was read from the 12(2019) text, so the purchase order should name the edition it invokes.

Fabrication Points for This Pair

Restore seams with a qualified nickel-molybdenum-chromium filler over the carbon steel and keep dilution low enough that the cap keeps its molybdenum and chromium levels.

Remove heat tint and contamination from the face after welding; keep carbon steel tools and grinding discs separate.

Bonding Process, Delivery and Heat Treatment

A265-12(2019) requires a condition appropriate to the cladding and/or the backing unless otherwise specified. B575 plate is supplied solution annealed, and a long hold in an intermediate temperature range can reduce the corrosion resistance of C276, so any post-bonding or post-weld cycle must be agreed and tested.

Manufacturing and delivery parameters for the enquiry
Parameter Order definition Engineering note
Bonding route Explosion bonded or hot-roll bonded Explosion bonding is common for C276 on thick backing
Layer thickness Backing gage plus minimum facing gage in mm; single- or double-sided Allow facing margin for grinding, forming and weld restoration; total gage alone does not define the plate.
Final thermal condition Named final condition and any simulated PWHT Represent fabrication cycles on coupons
Surface and edges Pickled or as agreed Face cleaned and protected
Lead time Confirmed against the enquiry Depends on plate area, layer gages, quantity, thermal condition and witnessed inspection.

Inspection and Certification

C276 clad plate inspection confirms the low carbon and silicon of the face, the A265 tests and any corrosion test the purchaser adds.

Inspection and test documents for the finished plate
Check What to specify Why it matters
Layer identity Separate backing and facing certificates with heat numbers No blended composite analysis
C and Si check Facing heat analysis against B575 limits Key alloy controls
Corrosion test Method and acceptance, if ordered Not automatic
Bond tests Shear or bond bend; ultrasonic acceptance level Interface and area
Tensile Composite or backing-only per A265 Section declared on report

Frequently Asked Questions

Where is C276 clad plate typically used?

Flue-gas desulfurization equipment, pickling lines, pulp bleaching and chemical vessels handling mixed or chloride-bearing acids.

What is the difference between C276 and Alloy 625 cladding?

C276 has much higher molybdenum and added tungsten for reducing acids and very aggressive chloride media. Alloy 625 contains niobium and more chromium. Selection follows the process chemistry.

Why is carbon limited to 0.010% in C276?

The very low carbon and silicon reduce grain-boundary precipitation in welds and heat-affected zones, helping maintain corrosion resistance after welding.

Can C276 clad plate receive post-weld heat treatment?

Only by agreement. The cycle must protect the alloy corrosion resistance and the backing properties, and should be represented on test coupons.

Is C22 the same as C276?

No. Alloy C22 is UNS N06022, also in B575, with different chromium, molybdenum and tungsten ranges. It must be ordered separately.

What minimum strength does the C276 face have?

B575-17(2023) gives 690 MPa tensile, 283 MPa yield and 40% elongation for N10276 plate. That is the alloy reference, not the clad-plate design value.

How thin can the C276 layer be if a shear test is required?

A265 identifies 0.075 in. (1.9 mm) facing for the shear test; testing at or below that needs agreement, or bond bend tests are used.

What details are needed for a C276 clad quotation?

A265 edition, backing grade and thickness, minimum C276 thickness, size, quantity, final condition, PWHT, bond and ultrasonic requirements and any corrosion test. Lead time is confirmed against the enquiry.

Related Materials

ASTM A265 nickel-alloy clad plate; A516 Grade 70 + Alloy 625 clad plate; all clad steel plate combinations.

Other Products