S355J2 EN 10025-2 equivalent: S355J2 (material number 1.0577) is a non-alloy structural steel with 355 MPa minimum yield and 27 J Charpy at −20°C. Its common equivalents are ASTM A572 Grade 50 (no impact requirement unless ordered), the old DIN 17100 St52-3, GB/T 1591 Q355D, UNI Fe 510 D and JIS SM490B. A572 Gr 50 is the usual US substitute, with 345 MPa yield and 450 MPa minimum tensile.

Gangsteel, a steel plate exporter, supplies EN 10025-2 S355J2 plate. Chemistry below is from EN 10025-2:2004, which gives both ladle and product analysis.

S355J2 chemical composition, % max (t ≤ 16 / 16–40 / >40 mm)

ElementLadle analysisProduct analysisASTM A572 Gr 50 (heat)
C0.20 / 0.20 / 0.220.23 / 0.23 / 0.240.23
Si0.550.600.40 (t ≤ 40 mm)
Mn1.601.701.35
P0.0250.0350.030
S0.0250.0350.030
Cu0.550.60–
N– (fully killed)––
CEV (t ≤ 30 / 30–40 mm)0.45 / 0.47––

Sources: EN 10025-2:2004 Tables 2, 3 and 6; ASTM A572/A572M Table 3 (Type 1–3 add Nb and/or V). EN 10025-2:2019 keeps the J2 limits at P 0.025, S 0.025.

ASTM A572 Gr 50 product analysis tolerances (ASTM A6/A6M)

ElementSpecified limit range, %Under minOver max
Cto 0.15 incl.0.020.03
C> 0.15 to 0.400.030.04
Mn> 0.60 to 0.900.060.08
Mn> 0.90 to 1.200.080.10
Mn> 1.20 to 1.350.090.11
Pto 0.040 incl.–0.010
Sto 0.060 incl.–0.010
Sito 0.30 incl.0.020.03
Si> 0.30 to 0.400.050.05
Cu (min specified)0.20 min0.02–
Vto 0.10 incl.0.010.01
V> 0.10 to 0.250.020.02
Nbto 0.10 incl.0.010.01

Source: ASTM A6/A6M, product analysis tolerances table. The product specification gives heat analysis; product (check) analysis may fall outside the heat limits by no more than these amounts.

Mechanical properties (t ≤ 16 mm)

PropertyS355J2ASTM A572 Gr 50
Yield, min355 MPa345 MPa (50 ksi)
Tensile470–630 MPa (t < 3 mm: 510–680)450 MPa (65 ksi) min
Elongation, min22% (long., 3–40 mm)18% in 200 mm; 21% in 50 mm
Charpy V, min27 J at −20°Cnot required (supplementary S5)

Sources: EN 10025-2 Tables 7 and 9; ASTM A572/A572M Table 4.

Related: EN 10025-2 S355J2 plate, ASTM A572 Grade 50 plate, GB/T 1591 Q355D plate.

 

 

equivalent of s355j2 en 10025-2 Overview of S355J2 EN 10025-2

 

S355J2 is a European standard grade for hot-rolled structural steels with a minimum yield strength of 355 MPa and impact at -20°C. Its equivalents include ASTM A572 Grade 50, used for similar applications worldwide. Our team offers S355J2 with equivalents like EN 10025-2 S355K2 steel and EN 10025-2 S450J0 steel, ensuring compliance for global projects.

 

equivalent of s355j2 en 10025-2 Grade Mapping

 

S355J2 EN 10025-2 has direct equivalents in other standards. The table below maps it to key grades:

Standard

Equivalent Grade

Notes

ASTM (USA)

A572 Grade 50

Similar strength for construction.

DIN (Germany)

ST52-3

Equivalent mechanical properties.

JIS (Japan)

SM490YA

For welded structures.

GB (China)

Q355D

Matches impact at -20°C.

NFA (France)

E36-3

For construction applications.

UNI (Italy)

Fe 510 D

Comparable tensile strength.

BS (UK)

50 C

For welded structures.

UNE (Spain)

AE 355 D

Similar characteristics.

Key Notes on Grade Mapping:

  • ASTM A572 Gr 50: Primary equivalent, with yield 345 MPa for high-strength use.
  • DIN ST52-3: Match for European projects.
  • JIS SM490YA: Good for Asian sourcing, with comparable weldability.
  • GB Q355D: Chinese equivalent for high-strength low-alloy needs.

These mappings are functional, but verify for specific codes. Our team provides dual-certified plates, including EN 10025-2 S235J2 steel and EN 10025-2 S355JR+N.

 

equivalent of s355j2 en 10025-2 Chemical Composition Comparison

 

Chemical compositions are similar, with low carbon for weldability. The table below compares S355J2 EN 10025-2 with ASTM A572 Gr 50 (% by weight, max values):

Key Notes on Chemical Composition:

  • S355J2 has stricter P/S for toughness.
  • ASTM A572 Gr 50 has broader limits but comparable weldability.

our plates meet multiple standards for easy equivalence.

 

equivalent of s355j2 en 10025-2 Mechanical Properties Comparison

 

Mechanical properties are close, with S355J2 offering specified impact at -20°C. The table below compares S355J2 EN 10025-2 with ASTM A572 Gr 50 (for plates up to 16 mm):

Key Notes on Mechanical Properties:

  • Both have similar strength, but EN 10025-2 guarantees impact.
  • ASTM A572 Gr 50 is versatile but may need testing for cold use.

Our team provides tested plates for reliable performance.

 

equivalent of s355j2 en 10025-2 Applications and Substitution Considerations

 

S355J2 EN 10025-2 is used in construction (bridges), offshore (platforms), and machinery (cranes). Its equivalent A572 Gr 50 substitutes for:

  • High-rise buildings and heavy bridges.
  • Wind turbines and moderate-cold machinery.

Substitution considerations:

  • Standards Compliance: EN for Europe, ASTM for US.
  • Toughness: EN has impact testing; ASTM may not.
  • Cost/Availability: ASTM in US, EN in Europe; our team bridges this.

For low-temperature, check EN 10025-2 S355J2 steel or EN 10025-2 S355K2 steel.

 

Why Choose Us for S355J2 EN 10025-2 Equivalents?

 

Our team is a trusted supplier of S355J2 EN 10025-2 equivalents, offering:

  • Certified Quality: Plates undergo ultrasonic testing and chemical analysis to meet EN/ASTM standards.
  • Customization: Available in thicknesses from 6–300 mm, with options for normalization.
  • Global Supply: Competitive pricing and reliable delivery worldwide.
  • Technical Support: Guidance on equivalents like EN 10025-2 S275J2 steel or EN 10025-2 S355JR+N.

 

Summary

 

The equivalent of S355J2 EN 10025-2 is ASTM A572 Grade 50, DIN ST52-3, JIS SM490YA, and GB Q355D, with similar high strength and low-temperature toughness for structural use. our high-quality plates ensure compliance for your projects. For more, explore our BS EN 10025-2 material grade guide.

More reading: EN 10025-2 S355J2

S355J2 EN 10025-2 Equivalent Grades FAQ

What is S355J2 equivalent to in ASTM?

ASTM A572 Grade 50 is the closest; specify supplementary Charpy testing at −20°C if you need S355J2-level toughness.

Is S355J2 the same as St52-3?

Practically yes. St52-3 from the withdrawn DIN 17100 was replaced by S355J2 (S355J2G3) in EN 10025.

What is the Chinese equivalent of S355J2?

GB/T 1591 Q355D, which is also impact tested at −20°C. Q355B is closer to S355JR.

What is the JIS equivalent of S355J2?

JIS G3106 SM490B is the usual match; SM490C has a 0°C impact test and SM490YB has a higher 365 MPa yield.

Is S355J2 the same as S355J2+N?

Same grade; +N means the plate is delivered normalized or normalized rolled, which is required for some sizes and specifications.

What is the difference between S355JR and S355J2?

Only the impact test temperature: JR is tested at +20°C and J2 at −20°C, with stricter P and S limits for J2.

What does 1.0577 mean?

1.0577 is the EN 10027-2 material number for S355J2.