RINA steel plate
RINA F420 Steel Plate | F420 Shipbuilding Steel Plate
RINA F420 steel plate, also written as RI/F420, RINA Grade F420, Registro Italiano Navale F420 or market names such as FH42 / FQ43, is the extra-high-strength hull structural steel of RINA Rules for the Classification of Ships (IACS UR W16 extra-high-strength family) with 420 MPa minimum yield, 530-680 MPa tensile strength and Charpy V-notch toughness at -60°C [-76°F]. In the grade name, "F" is the toughness class, and "420" is the yield-strength level in MPa (not AH420). Gangsteel, a steel plate exporter, supplies RINA F420 / RI/F420 plates cut to size for shipbuilding, offshore platforms and marine structures.
Data source: Per IACS UR W16 (extra-high-strength hull structural steel) as adopted in RINA (Registro Italiano Navale) hull structural steel rules, cross-checked with LR FH42 / ABS FQ43 sibling pages on gangsteel.net. Official mill/certificate grade is RINA F420 (RI/F420). Verify the current RINA edition before ordering.
RINA F420 Chemical Composition (Heat Analysis)
| Element | C | Mn | Si | P | S | Al (acid sol.) |
|---|---|---|---|---|---|---|
| RINA F420, % | 0.18 max | 1.60 max | 0.10-0.55 | 0.025 max | 0.025 max | 0.015 min |
| Element | N | Nb | V | Ti | B | Notes |
| RINA F420, % | 0.020 max | 0.02-0.05 | 0.04-0.10 | 0.02 max | 0.005 max | Ni/Cu/Cr/Mo per delivery condition (N/TM/QT) in UR W16 |
Per IACS UR W16 / RINA extra-high-strength rules. Exact maxima for Ni, Cu, Cr and Mo depend on delivery condition (N/NR, TM or QT). Carbon equivalent / CET / Pcm limits apply by thickness and condition; confirm on the mill certificate and current rule edition.
Product Analysis (Check Analysis)
When product analysis is required, apply ASTM A6/A6M Table A permitted variations to the heat limits unless the element is min-only or not listed in Table A.
| Element | Heat analysis limit | Product analysis (heat ± A6) |
|---|---|---|
| C | 0.18 max | 0.22 max |
| Mn | 1.60 max | see A6 Table A vs heat upper limit |
| Si | 0.10-0.55 | 0.05–0.61 (approx. A6) |
| P | 0.025 max | 0.035 max |
| S | 0.025 max | 0.035 max |
| Al (acid sol.) | 0.015 min | no A6 Table A tolerance; product value not tabulated |
| N | 0.020 max | 0.025 max (typical A6 +0.005) |
| Nb | 0.02-0.05 | 0.010–0.060 |
| V | 0.04-0.10 | 0.030–0.110 |
| Ti | 0.02 max | 0.03 max |
| B | 0.005 max | product analysis often not applicable |
Product analysis applies only when specified; for a range, results may not vary both above and below it.
RINA F420 Mechanical Properties
| Grade | Yield strength, min | Tensile strength | Elongation, min |
|---|---|---|---|
| RINA F420 | 420 MPa [61 ksi] | 530-680 MPa [77-99 ksi] | 18% |
Per IACS UR W16 / RINA rules (common t≤50 mm values). Yield may step down for thicker plates per UR W16; confirm thickness-dependent values on the order.
Charpy V-Notch Impact Requirements (-60°C [-76°F])
| Thickness | Test temperature | Longitudinal, avg min | Transverse, avg min |
|---|---|---|---|
| t≤50 mm | -60°C [-76°F] | 42 J | 28 J |
| 50<t≤70 mm | -60°C [-76°F] | 42 J | 28 J |
| 70<t≤100 mm | -60°C [-76°F] | 42 J | 28 J |
Per IACS UR W16 / RINA extra-high-strength practice. Average of three full-size specimens; transverse values apply when required. Thicker plates by agreement.
Delivery Condition and Deoxidation
Deoxidation: Killed, fine-grain practice. Delivery condition: typically TMCP or QT for extra-high-strength plates; N/NR may apply at lower extra-high levels per rules. F-class (F420) grades are supplied normalized or TMCP (often with Ni alloying for -60°C toughness); as-rolled delivery is not permitted. Optional extras: UT, Z15/Z25/Z35, RINA survey.
Thickness Coverage
Extra-high-strength RINA A/D/E/F 420-690 plates are commonly supplied from about 6 mm to 100 mm thick (thicker by agreement under UR W16). Width 1500-4000 mm and length 6000-18000 mm are typical.
Equivalent Steel Grades of RINA F420
| Society / Standard | Equivalent grade |
|---|---|
| RINA (Registro Italiano Navale) | RINA F420 steel plate (RI/F420; LR FH42 / ABS FQ43) |
| LR (Lloyd's Register) | LR FH42 steel plate |
| CCS | CCS F420 steel plate |
| GL | GL F420 steel plate |
| DNV | DNV F420 steel plate |
| NK | NK F43 steel plate |
| KR | KR F43 steel plate |
| BV | BV F420 steel plate |
IACS societies align extra-high-strength hull grades under UR W16; naming differs (RINA F420, LR FH42, ABS FQ43). Dual certification is common when ordered that way.
FAQ about RINA F420 Steel Plate
What is RINA F420 steel plate?
It is an extra-high-strength hull structural steel under RINA Rules (IACS UR W16 extra-high-strength family), with 420 MPa minimum yield, 530-680 MPa tensile strength and Charpy toughness at -60°C [-76°F]. The mill certificate grade is RINA F420 (RI/F420).
What does RINA F420 / RI/F420 stand for?
RINA is Registro Italiano Navale (RI on certificates). The letter F is the toughness class (Charpy at -60°C [-76°F]), and 420 is the yield-strength level in MPa. Market/LR naming often uses FH42; ABS often uses FQ43. Note: RINA does not use AH420 — the grade is F420, not AH420.
What is the yield strength of RINA F420?
Minimum 420 MPa (61 ksi), tensile 530-680 MPa (77-99 ksi), elongation about 18% min (for the common thickness range).
What is the impact test temperature for RINA F420?
Charpy V-notch at -60°C [-76°F]. Typical longitudinal average minimum is 42 J (transverse 28 J) for the tabulated thickness range on this grade page.
What is the difference between RINA A420, D420, E420 and F420?
Same 420 MPa strength class. Toughness class differs: A at 0°C, D at -20°C, E at -40°C, F at -60°C. Chemistry (C, P, S, Mn) is tightened for colder classes.
How does RINA F420 differ from higher-strength RINA AH40?
RINA AH40 is UR W11 higher-strength (390 MPa). RINA F420 is UR W16 extra-high-strength (420 MPa) with different chemistry and delivery practice (often TM/QT).
Is RINA F420 the same as LR FH42 or ABS FQ43?
They are IACS counterparts in the extra-high-strength family; exact chemistry/delivery options differ by society edition. Dual certification is available when surveys are arranged.
Is RINA F420 weldable?
Weldable with approved procedures for extra-high-strength ship steel. Preheat, heat input and consumable matching are critical; follow the mill WPS and RINA welding requirements.
What heat treatment is required for RINA F420?
Extra-high-strength grades are typically delivered TMCP or quenched and tempered (QT), sometimes normalized/normalized-rolled depending on strength level and thickness. F-class (F420) grades are supplied normalized or TMCP (often with Ni alloying for -60°C toughness); as-rolled delivery is not permitted. Optional extras: UT, Z15/Z25/Z35, RINA survey.
What thickness is available for RINA F420?
Common supply is about 6-100 mm (thicker by agreement under UR W16 / RINA rules), 1500-4000 mm wide and 6000-18000 mm long.
Other RINA Steel Plate Grades
RINA Grade A steel plate | RINA Grade B steel plate | RINA Grade D steel plate | RINA Grade E steel plate | RINA AH32 steel plate | RINA AH36 steel plate | RINA AH40 steel plate | RINA DH32 steel plate | RINA DH36 steel plate | RINA DH40 steel plate | RINA EH32 steel plate | RINA EH36 steel plate | RINA EH40 steel plate | RINA FH32 steel plate | RINA FH36 steel plate | RINA FH40 steel plate | RINA A420 steel plate | RINA A460 steel plate | RINA A500 steel plate | RINA A550 steel plate | RINA A620 steel plate | RINA A690 steel plate | RINA D420 steel plate | RINA D460 steel plate | RINA D500 steel plate | RINA D550 steel plate | RINA D620 steel plate | RINA D690 steel plate | RINA E420 steel plate | RINA E460 steel plate | RINA E500 steel plate | RINA E550 steel plate | RINA E620 steel plate | RINA E690 steel plate | RINA F460 steel plate | RINA F500 steel plate | RINA F550 steel plate | RINA F620 steel plate | RINA F690 steel plate
Equivalent Class Society Grades
RINA F420 corresponds to extra-high-strength counterparts under other IACS societies (LR FH42, ABS FQ43, etc.): LR FH42 steel plate, CCS F420 steel plate, GL F420 steel plate, DNV F420 steel plate, NK F43 steel plate, KR F43 steel plate, BV F420 steel plate, RINA F420 steel plate.
-
RINA DH36 Steel Plate | DH36 Sh
RINA DH36 (RI/DH36) shipbuilding steel plate: 355 MPa yield, 490-620 MPa tensile, Charpy at -20C, chemistry and
-
RINA AH36 Steel Plate | AH36 Sh
RINA AH36 (RI/AH36) shipbuilding steel plate: 355 MPa yield, 490-620 MPa tensile, Charpy at 0C, chemistry and e
-
RINA FH32 Steel Plate | FH32 Sh
RINA FH32 (RI/FH32) shipbuilding steel plate: 315 MPa yield, 440-590 MPa tensile, Charpy at -60C, chemistry and
-
RINA Grade A Steel Plate | Grad
RINA Grade A (RI/A) shipbuilding steel plate: 235 MPa yield, 400-520 MPa tensile, Charpy at +20C, chemistry and