What an S275JR HE Beam Order Specifies
S275JR sits between S235 and S355 in EN 10025-2: 275 MPa minimum yield for thin products, a +20 °C impact quality and a moderate carbon equivalent. Supplied as HE A or HE B beams to EN 10365, it suits frames where S235 would require a heavier section but S355 is not needed. Enquiries to Gangsteel should quote the full HE designation together with EN 10025-2 S275JR.
S275 has long been a default structural grade in several markets because it improves member resistance over S235 while keeping welding procedures straightforward. Whether it is the economic choice for a given HE section depends on design governing criteria, which the project engineer decides.
| Item | Value for this product | Comment |
|---|---|---|
| Material standard | EN 10025-2:2019 | Non-alloy structural steel, hot-rolled products |
| Steel name / number | S275JR / 1.0044 | Quality JR: impact test temperature in the table below |
| Section series and dimensions | HE A and HE B to EN 10365:2017 | Geometry and nominal mass only; no strength content |
| Shape and dimensional tolerances | EN 10034 | Acceptance of depth, width, thickness, squareness and straightness |
| General delivery requirements | EN 10025-1 | Testing, inspection documents and marking rules shared by the EN 10025 parts |
| Former national designation | St 44-2 (DIN 17100, withdrawn) | Historical reference only |
HE A and HE B Sizes Read Through the S275JR Thickness Bands
EN 10365 fixes the geometry; EN 10025-2 fixes how strong the material must be at a given product thickness. For sections, tensile test pieces are normally taken from the flange, so the flange thickness tf is the practical reference for choosing the applicable S275JR band. The tables combine both: nominal HE A or HE B dimensions on the left, and on the right the minimum upper yield strength that the S275JR table requires at that flange thickness. The rows are reference geometry, not a stock list.
| Section | h mm | b mm | tw mm | tf mm | kg/m | Min. ReH MPa |
|---|---|---|---|---|---|---|
| HE 100 A | 96 | 100 | 5 | 8 | 16.7 | 275 |
| HE 120 A | 114 | 120 | 5 | 8 | 19.9 | 275 |
| HE 140 A | 133 | 140 | 5.5 | 8.5 | 24.7 | 275 |
| HE 160 A | 152 | 160 | 6 | 9 | 30.4 | 275 |
| HE 180 A | 171 | 180 | 6 | 9.5 | 35.5 | 275 |
| HE 200 A | 190 | 200 | 6.5 | 10 | 42.3 | 275 |
| HE 220 A | 210 | 220 | 7 | 11 | 50.5 | 275 |
| HE 240 A | 230 | 240 | 7.5 | 12 | 60.3 | 275 |
| HE 260 A | 250 | 260 | 7.5 | 12.5 | 68.2 | 275 |
| HE 280 A | 270 | 280 | 8 | 13 | 76.4 | 275 |
| HE 300 A | 290 | 300 | 8.5 | 14 | 88.3 | 275 |
| HE 320 A | 310 | 300 | 9 | 15.5 | 97.6 | 275 |
| HE 340 A | 330 | 300 | 9.5 | 16.5 | 105 | 265 |
| HE 360 A | 350 | 300 | 10 | 17.5 | 112 | 265 |
| HE 400 A | 390 | 300 | 11 | 19 | 125 | 265 |
| HE 450 A | 440 | 300 | 11.5 | 21 | 140 | 265 |
| HE 500 A | 490 | 300 | 12 | 23 | 155 | 265 |
| HE 550 A | 540 | 300 | 12.5 | 24 | 166 | 265 |
| HE 600 A | 590 | 300 | 13 | 25 | 178 | 265 |
| HE 650 A | 640 | 300 | 13.5 | 26 | 190 | 265 |
| HE 700 A | 690 | 300 | 14.5 | 27 | 204 | 265 |
| HE 800 A | 790 | 300 | 15 | 28 | 224 | 265 |
| HE 900 A | 890 | 300 | 16 | 30 | 252 | 265 |
| HE 1000 A | 990 | 300 | 16.5 | 31 | 272 | 265 |
| Section | h mm | b mm | tw mm | tf mm | kg/m | Min. ReH MPa |
|---|---|---|---|---|---|---|
| HE 100 B | 100 | 100 | 6 | 10 | 20.4 | 275 |
| HE 120 B | 120 | 120 | 6.5 | 11 | 26.7 | 275 |
| HE 140 B | 140 | 140 | 7 | 12 | 33.7 | 275 |
| HE 160 B | 160 | 160 | 8 | 13 | 42.6 | 275 |
| HE 180 B | 180 | 180 | 8.5 | 14 | 51.2 | 275 |
| HE 200 B | 200 | 200 | 9 | 15 | 61.3 | 275 |
| HE 220 B | 220 | 220 | 9.5 | 16 | 71.5 | 275 |
| HE 240 B | 240 | 240 | 10 | 17 | 83.2 | 265 |
| HE 260 B | 260 | 260 | 10 | 17.5 | 93.0 | 265 |
| HE 280 B | 280 | 280 | 10.5 | 18 | 103 | 265 |
| HE 300 B | 300 | 300 | 11 | 19 | 117 | 265 |
| HE 320 B | 320 | 300 | 11.5 | 20.5 | 127 | 265 |
| HE 340 B | 340 | 300 | 12 | 21.5 | 134 | 265 |
| HE 360 B | 360 | 300 | 12.5 | 22.5 | 142 | 265 |
| HE 400 B | 400 | 300 | 13.5 | 24 | 155 | 265 |
| HE 450 B | 450 | 300 | 14 | 26 | 171 | 265 |
| HE 500 B | 500 | 300 | 14.5 | 28 | 187 | 265 |
| HE 550 B | 550 | 300 | 15 | 29 | 199 | 265 |
| HE 600 B | 600 | 300 | 15.5 | 30 | 212 | 265 |
| HE 650 B | 650 | 300 | 16 | 31 | 225 | 265 |
| HE 700 B | 700 | 300 | 17 | 32 | 241 | 265 |
| HE 800 B | 800 | 300 | 17.5 | 33 | 262 | 265 |
| HE 900 B | 900 | 300 | 18.5 | 35 | 291 | 265 |
| HE 1000 B | 1000 | 300 | 19 | 36 | 314 | 265 |
h is overall depth, b flange width, tw web thickness and tf flange thickness; kg/m is nominal mass. HE A is the lighter series for the same serial size and HE B the heavier one: HE 300 A is 290 mm deep with a 14 mm flange, while HE 300 B is 300 mm deep with a 19 mm flange. Order the full designation, because a drawing note such as “H300” does not distinguish them.
The 16 mm flange threshold again divides the series. HE 100 A to HE 320 A and HE 100 B to HE 220 B fall in the 275 MPa band; HE 340 A to HE 1000 A and HE 240 B to HE 1000 B fall in the 265 MPa band. Carbon (0.21%) and CEV (0.40%) do not change anywhere in the HE A and HE B tables, because the next thickness step for those limits is above 40 mm.
S275JR Chemical Composition for HE Sections
| Element | Maximum | How it applies to HE A / HE B |
|---|---|---|
| C | 0.21 | 0.21 up to 40 mm; 0.22 above 40 mm (not reached by HE A/HE B) |
| Mn | 1.50 | — |
| Si | — | No maximum in this grade row; a galvanizing range may be agreed |
| P | 0.040 | 0.035 may be agreed with the galvanizing silicon option |
| S | 0.040 | — |
| N | 0.012 | Waived with total Al ≥ 0.020% or sufficient reported nitrogen-binding elements |
| Cu | 0.55 | — |
| CEV | 0.40 | Up to 40 mm; 0.42 above 40 mm. Special S275 provisions of EN 10025-2:2019 clause 7.2.5 apply where invoked |
Compared with S235JR, S275JR allows more carbon (0.21% against 0.17%) and manganese (1.50% against 1.40%), which together raise strength and the CEV ceiling from 0.35% to 0.40%. EN 10025-2:2019 clause 7.2.5 contains special provisions for S275 that the purchaser may invoke; if they are required, they must appear in the order.
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Cu + Ni)/15, using heat-analysis values. Additional elements, if added, must be stated on the inspection document. These are limits for acceptance, not the composition of any particular heat.
S275JR Mechanical Properties by Flange Thickness
| Property | tf ≤ 16 mm | 16 mm < tf ≤ 40 mm |
|---|---|---|
| Minimum upper yield strength ReH | 275 MPa | 265 MPa |
| Tensile strength Rm | 410–560 MPa | 410–560 MPa |
| Minimum elongation A, L0 = 5.65√S0 | 23% | 23% |
| Charpy V-notch, minimum | 27 J at +20 °C | 27 J at +20 °C |
The tensile range of 410–560 MPa and the 23% elongation are distinct from both neighbouring grades. As with every JR quality, the impact requirement is at +20 °C only.
How S275JR Differs from Neighbouring EN 10025-2 Grades
| Grade | Key difference from S275JR | Ordering consequence |
|---|---|---|
| S235JR | Yield 235/225 MPa; C 0.17%; CEV 0.35% | Lower resistance per HE size; easier to obtain in some markets |
| S275J0 / S275J2 | Same strength; impact at 0 °C / −20 °C; C limit 0.18% and tighter P and S | A JR certificate does not satisfy a J0 or J2 order |
| S355JR | Yield 355/345 MPa; C 0.24%; CEV 0.45/0.47% | Higher resistance; different design and welding data |
Gangsteel supplies EN 10025-2 S275JR HEA and HEB beams. Exact size, quantity, delivery condition and lead time are confirmed per enquiry, and the grade, flange-thickness band and certificate wording should be stated for each size on the order.
Welding, Cutting and Galvanizing Notes
A CEV of 0.40% still gives good weldability for HE flanges up to 36 mm, but thicker flanges combined with high restraint can call for preheat assessment under the welding standard used. Cutting and drilling behave like other non-alloy structural grades. For galvanizing, the agreed silicon range and P ≤ 0.035% option applies to S275JR in the same way as to S235JR.
Delivery Condition, Heat Treatment and Inspection
| Item | What to specify | Why it matters |
|---|---|---|
| Delivery condition | As-rolled (+AR) or normalized / normalizing rolled (+N) where the order requires it | The grade name alone does not fix the delivery condition; +N must be ordered explicitly |
| Heat treatment after delivery | Normally none for rolled HE beams; any hot forming or stress relief needs an agreed procedure | Uncontrolled heating can alter the certified properties |
| Impact verification | State whether the 27 J at +20 °C test is to be verified and reported | Avoids a certificate that lists the grade but no Charpy result |
| Inspection document | EN 10204 type, typically 3.1 when specific test results are required | Results must be traceable to the heat and the delivered pieces |
| Dimensional acceptance | EN 10034 tolerances, length tolerance and cut-length list | Nominal table values are not tolerance limits |
Specify whether the +20 °C impact result must be reported. Where the purchaser invokes the clause 7.2.5 special S275 requirements, quote them in the purchase order and check them on the certificate.
RFQ Checklist for S275JR HEA and HEB Beams
- Full section designation, for example HE 300 B, not “H300”.
- Material as EN 10025-2 S275JR, with delivery condition and any options such as galvanizing chemistry.
- Lengths, quantities and total mass basis (theoretical or weighed).
- Impact verification, EN 10204 document type and heat traceability.
- Cutting, drilling, blasting or coating drawings, packing and destination.
Typical lead time is about 35 days for mill orders; sizes available from stock can ship in 1-3 days. Stock availability by size is confirmed at enquiry; the tables on this page are reference geometry, not a stock list.
For flat components in the same structure, order EN 10025-2 S275JR steel plate separately; plate and section certificates are issued per product. For the narrow-flange alternative see the EN 10365 IPE beam range with EN 10025-2 grades, and for heavier column sections the universal column (UC) range. The structural steel sections selection guide compares the families.
Other EN 10025-2 grades in the same HE A / HE B series: S235JR HEA and HEB beams, S355JR HEA and HEB beams, S355J2 HEA and HEB beams.
Frequently Asked Questions
When is S275JR chosen over S235JR for HE beams?
When the engineer needs more resistance from the same HE size, or wants a lighter size while staying with a moderate CEV. The improvement is about 17% in minimum yield for thin flanges. Whether that saves steel depends on whether strength, stability or deflection governs.
At which HE size does the S275JR yield drop to 265 MPa?
When the flange exceeds 16 mm: from HE 340 A in the A series and from HE 240 B in the B series. Using 275 MPa for those sections overstates the guaranteed minimum.
Can Gangsteel supply S275JR HEA and HEB beams?
Yes. Gangsteel supplies EN 10025-2 S275JR HEA and HEB beams. Exact size, quantity, delivery condition and lead time are confirmed per enquiry; not every size is necessarily held in stock, so state the full HE designation, length and quantity in the RFQ.
What does the JR in S275JR mean?
JR is the impact quality: a minimum of 27 J in a Charpy V-notch test at +20 °C. It does not demonstrate toughness at lower temperatures; S275J0 and S275J2 are the colder-test qualities and must be ordered by name.
Can S355JR be delivered instead of S275JR?
Only if the purchaser and design engineer accept it. Higher strength is not automatically better: connection design, weld procedures and certificates are tied to the specified grade. Silent substitution is not appropriate for certified structural work.
What are the S275 special provisions in EN 10025-2?
Clause 7.2.5 of EN 10025-2:2019 sets special requirements that the purchaser may invoke for S275 and S355. They are not automatic; if needed, they must be written into the order and verified on the inspection document.
Is S275JR suitable for hot-dip galvanizing?
Yes, when the galvanizing chemistry option is agreed: silicon in the range 0.14 to 0.25% and phosphorus not above 0.035%. Without that option, silicon in the reactive range can produce excessive coating thickness.