What an S355JR HE Beam Order Specifies
S355JR is the 355 MPa grade of EN 10025-2 with the least demanding impact quality, tested at +20 °C. In HE A and HE B beams it is used where strength-governed members benefit from higher yield but low-temperature toughness is not specified. Enquiries to Gangsteel should state the exact HE designation and EN 10025-2 S355JR.
Two things set S355JR apart on HE sections: the yield band, which drops from 355 to 345 MPa above a 16 mm flange, and the carbon equivalent, which rises from 0.45% to 0.47% above 30 mm. Both are visible in the size tables below.
| Item | Value for this product | Comment |
|---|---|---|
| Material standard | EN 10025-2:2019 | Non-alloy structural steel, hot-rolled products |
| Steel name / number | S355JR / 1.0045 | Quality JR: impact test temperature in the table below |
| Section series and dimensions | HE A and HE B to EN 10365:2017 | Geometry and nominal mass only; no strength content |
| Shape and dimensional tolerances | EN 10034 | Acceptance of depth, width, thickness, squareness and straightness |
| General delivery requirements | EN 10025-1 | Testing, inspection documents and marking rules shared by the EN 10025 parts |
| Former designation | Fe 510 B (EN 10025:1990) | Historical reference only |
HE A and HE B Sizes Read Through the S355JR Thickness Bands
EN 10365 fixes the geometry; EN 10025-2 fixes how strong the material must be at a given product thickness. For sections, tensile test pieces are normally taken from the flange, so the flange thickness tf is the practical reference for choosing the applicable S355JR band. The tables combine both: nominal HE A or HE B dimensions on the left, and on the right the minimum upper yield strength that the S355JR table requires at that flange thickness. The rows are reference geometry, not a stock list.
| Section | h mm | b mm | tw mm | tf mm | kg/m | Min. ReH MPa | CEV max % |
|---|---|---|---|---|---|---|---|
| HE 100 A | 96 | 100 | 5 | 8 | 16.7 | 355 | 0.45 |
| HE 120 A | 114 | 120 | 5 | 8 | 19.9 | 355 | 0.45 |
| HE 140 A | 133 | 140 | 5.5 | 8.5 | 24.7 | 355 | 0.45 |
| HE 160 A | 152 | 160 | 6 | 9 | 30.4 | 355 | 0.45 |
| HE 180 A | 171 | 180 | 6 | 9.5 | 35.5 | 355 | 0.45 |
| HE 200 A | 190 | 200 | 6.5 | 10 | 42.3 | 355 | 0.45 |
| HE 220 A | 210 | 220 | 7 | 11 | 50.5 | 355 | 0.45 |
| HE 240 A | 230 | 240 | 7.5 | 12 | 60.3 | 355 | 0.45 |
| HE 260 A | 250 | 260 | 7.5 | 12.5 | 68.2 | 355 | 0.45 |
| HE 280 A | 270 | 280 | 8 | 13 | 76.4 | 355 | 0.45 |
| HE 300 A | 290 | 300 | 8.5 | 14 | 88.3 | 355 | 0.45 |
| HE 320 A | 310 | 300 | 9 | 15.5 | 97.6 | 355 | 0.45 |
| HE 340 A | 330 | 300 | 9.5 | 16.5 | 105 | 345 | 0.45 |
| HE 360 A | 350 | 300 | 10 | 17.5 | 112 | 345 | 0.45 |
| HE 400 A | 390 | 300 | 11 | 19 | 125 | 345 | 0.45 |
| HE 450 A | 440 | 300 | 11.5 | 21 | 140 | 345 | 0.45 |
| HE 500 A | 490 | 300 | 12 | 23 | 155 | 345 | 0.45 |
| HE 550 A | 540 | 300 | 12.5 | 24 | 166 | 345 | 0.45 |
| HE 600 A | 590 | 300 | 13 | 25 | 178 | 345 | 0.45 |
| HE 650 A | 640 | 300 | 13.5 | 26 | 190 | 345 | 0.45 |
| HE 700 A | 690 | 300 | 14.5 | 27 | 204 | 345 | 0.45 |
| HE 800 A | 790 | 300 | 15 | 28 | 224 | 345 | 0.45 |
| HE 900 A | 890 | 300 | 16 | 30 | 252 | 345 | 0.45 |
| HE 1000 A | 990 | 300 | 16.5 | 31 | 272 | 345 | 0.47 |
| Section | h mm | b mm | tw mm | tf mm | kg/m | Min. ReH MPa | CEV max % |
|---|---|---|---|---|---|---|---|
| HE 100 B | 100 | 100 | 6 | 10 | 20.4 | 355 | 0.45 |
| HE 120 B | 120 | 120 | 6.5 | 11 | 26.7 | 355 | 0.45 |
| HE 140 B | 140 | 140 | 7 | 12 | 33.7 | 355 | 0.45 |
| HE 160 B | 160 | 160 | 8 | 13 | 42.6 | 355 | 0.45 |
| HE 180 B | 180 | 180 | 8.5 | 14 | 51.2 | 355 | 0.45 |
| HE 200 B | 200 | 200 | 9 | 15 | 61.3 | 355 | 0.45 |
| HE 220 B | 220 | 220 | 9.5 | 16 | 71.5 | 355 | 0.45 |
| HE 240 B | 240 | 240 | 10 | 17 | 83.2 | 345 | 0.45 |
| HE 260 B | 260 | 260 | 10 | 17.5 | 93.0 | 345 | 0.45 |
| HE 280 B | 280 | 280 | 10.5 | 18 | 103 | 345 | 0.45 |
| HE 300 B | 300 | 300 | 11 | 19 | 117 | 345 | 0.45 |
| HE 320 B | 320 | 300 | 11.5 | 20.5 | 127 | 345 | 0.45 |
| HE 340 B | 340 | 300 | 12 | 21.5 | 134 | 345 | 0.45 |
| HE 360 B | 360 | 300 | 12.5 | 22.5 | 142 | 345 | 0.45 |
| HE 400 B | 400 | 300 | 13.5 | 24 | 155 | 345 | 0.45 |
| HE 450 B | 450 | 300 | 14 | 26 | 171 | 345 | 0.45 |
| HE 500 B | 500 | 300 | 14.5 | 28 | 187 | 345 | 0.45 |
| HE 550 B | 550 | 300 | 15 | 29 | 199 | 345 | 0.45 |
| HE 600 B | 600 | 300 | 15.5 | 30 | 212 | 345 | 0.45 |
| HE 650 B | 650 | 300 | 16 | 31 | 225 | 345 | 0.47 |
| HE 700 B | 700 | 300 | 17 | 32 | 241 | 345 | 0.47 |
| HE 800 B | 800 | 300 | 17.5 | 33 | 262 | 345 | 0.47 |
| HE 900 B | 900 | 300 | 18.5 | 35 | 291 | 345 | 0.47 |
| HE 1000 B | 1000 | 300 | 19 | 36 | 314 | 345 | 0.47 |
h is overall depth, b flange width, tw web thickness and tf flange thickness; kg/m is nominal mass. HE A is the lighter series for the same serial size and HE B the heavier one: HE 300 A is 290 mm deep with a 14 mm flange, while HE 300 B is 300 mm deep with a 19 mm flange. Order the full designation, because a drawing note such as “H300” does not distinguish them.
For S355JR, HE 100 A to HE 320 A and HE 100 B to HE 220 B are in the 355 MPa band; larger sizes are at 345 MPa. The CEV maximum is 0.45% for flanges up to 30 mm and 0.47% above: in the listed series this affects HE 1000 A (31 mm) and HE 650 B to HE 1000 B (31–36 mm). Carbon remains 0.24% throughout.
S355JR Chemical Composition for HE Sections
| Element | Maximum | How it applies to HE A / HE B |
|---|---|---|
| C | 0.24 | Same maximum in every thickness band up to 100 mm |
| Si | 0.55 | — |
| Mn | 1.60 | — |
| P | 0.040 | 0.035 may be agreed with the galvanizing silicon option |
| S | 0.040 | — |
| N | 0.012 | Waived with total Al ≥ 0.020% or sufficient reported nitrogen-binding elements |
| Cu | 0.55 | — |
| CEV | 0.45 / 0.47 | 0.45 up to 30 mm; 0.47 for 30 mm < t ≤ 40 mm. Special S355 provisions of clause 7.2.5 apply where invoked |
S355JR has the highest carbon allowance of the 355 grades (0.24%), and the JR quality does not require fully killed practice in the way J2 does. Phosphorus and sulfur are each limited to 0.040%. The nitrogen limit of 0.012% is waived only where enough aluminium or other nitrogen-binding elements are present and reported.
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Cu + Ni)/15, using heat-analysis values. Additional elements, if added, must be stated on the inspection document. These are limits for acceptance, not the composition of any particular heat.
S355JR Mechanical Properties by Flange Thickness
| Property | tf ≤ 16 mm | 16 mm < tf ≤ 40 mm |
|---|---|---|
| Minimum upper yield strength ReH | 355 MPa | 345 MPa |
| Tensile strength Rm | 470–630 MPa | 470–630 MPa |
| Minimum elongation A, L0 = 5.65√S0 | 22% | 22% |
| Charpy V-notch, minimum | 27 J at +20 °C | 27 J at +20 °C |
The +20 °C impact quality is the main reason designers move from S355JR to S355J0 or S355J2 for external or cold-climate structures. JR material is commonly ordered for internal, heated buildings; the choice belongs to the design engineer and the applicable code.
How S355JR Differs from Neighbouring EN 10025-2 Grades
| Grade | Key difference from S355JR | Ordering consequence |
|---|---|---|
| S355J0 | Impact test at 0 °C; C 0.20/0.22%; P and S 0.035% | Colder test and tighter chemistry |
| S355J2 | Impact test at −20 °C; fully killed; P and S 0.030%; C 0.20/0.22% | A JR certificate cannot satisfy a J2 order |
| S275JR | Yield 275/265 MPa; CEV 0.40% | Lower resistance; different design values |
| ASTM A992 | Different standard family with a yield range of 50–65 ksi and Fy/Fu control | Not an equivalent label; see ASTM A992 wide flange W-beams for that material |
Strength class alone does not make grades interchangeable. The impact quality, chemistry and certificate requirements are part of the specification.
Welding, Cutting and Galvanizing Notes
With CEV up to 0.45–0.47%, S355JR HE beams need more attention to welding procedure than S235 or S275: preheat may be required for thick flanges, high restraint or low heat input, according to the welding standard and consumable data. The higher carbon allowance compared with S355J2 also matters for hardness in the heat-affected zone. Thermal cutting edges of thick flanges may need preparation before welding. The galvanizing chemistry option is available as for the other JR grades.
Delivery Condition, Heat Treatment and Inspection
| Item | What to specify | Why it matters |
|---|---|---|
| Delivery condition | As-rolled (+AR) or normalized / normalizing rolled (+N) where the order requires it | The grade name alone does not fix the delivery condition; +N must be ordered explicitly |
| Heat treatment after delivery | Normally none for rolled HE beams; any hot forming or stress relief needs an agreed procedure | Uncontrolled heating can alter the certified properties |
| Impact verification | State whether the 27 J at +20 °C test is to be verified and reported | Avoids a certificate that lists the grade but no Charpy result |
| Inspection document | EN 10204 type, typically 3.1 when specific test results are required | Results must be traceable to the heat and the delivered pieces |
| Dimensional acceptance | EN 10034 tolerances, length tolerance and cut-length list | Nominal table values are not tolerance limits |
Where the CEV of thicker HE B sizes matters to the welding procedure, ask for the actual heat CEV on the certificate rather than relying on the maximum.
RFQ Checklist for S355JR HEA and HEB Beams
- Full section designation, for example HE 300 B, not “H300”.
- Material as EN 10025-2 S355JR, with delivery condition and any options such as galvanizing chemistry.
- Lengths, quantities and total mass basis (theoretical or weighed).
- Impact verification, EN 10204 document type and heat traceability.
- Cutting, drilling, blasting or coating drawings, packing and destination.
Typical lead time is about 35 days for mill orders; sizes available from stock can ship in 1-3 days. Stock availability by size is confirmed at enquiry; the tables on this page are reference geometry, not a stock list.
For flat components in the same structure, order EN 10025-2 S355JR steel plate separately; plate and section certificates are issued per product. For the narrow-flange alternative see the EN 10365 IPE beam range with EN 10025-2 grades, and for heavier column sections the universal column (UC) range. The structural steel sections selection guide compares the families.
Other EN 10025-2 grades in the same HE A / HE B series: S235JR HEA and HEB beams, S275JR HEA and HEB beams, S355J2 HEA and HEB beams.
Frequently Asked Questions
Why does the S355JR CEV limit change within the HE B series?
EN 10025-2 sets a CEV maximum of 0.45% up to 30 mm and 0.47% for 30 mm to 40 mm. HE 650 B to HE 1000 B have flanges of 31 to 36 mm, so the higher limit applies to them, as it does to HE 1000 A.
Is S355JR suitable for outdoor steelwork?
It depends on the service temperature and the design code. JR is tested at +20 °C only. For structures exposed to low temperatures, engineers often specify S355J0 or S355J2. The decision belongs to the designer, not to the supplier.
What is the difference between S355JR and S355J2 HE beams?
The strength requirements are the same, but J2 is impact-tested at minus 20 °C, is fully killed with nitrogen-binding elements, and has tighter phosphorus and sulfur limits and a lower carbon maximum. The certificates are not interchangeable.
At which sizes is S355JR yield 345 MPa?
Where the flange exceeds 16 mm: HE 340 A and larger, and HE 240 B and larger. Design and acceptance should use the band that matches the flange thickness.
Is S355JR equivalent to ASTM A992?
No. They belong to different standard systems with different chemistry, tensile and impact requirements. A992 has a yield range and yield-to-tensile limit that S355JR does not; S355JR has an EN impact quality that A992 does not define in the same way. A project must order the specified standard.
Does S355JR need preheat for welding?
Not always. The need depends on CEV, flange thickness, joint restraint, heat input and hydrogen control, assessed under the welding standard used. Thick HE B flanges at the 0.47% CEV level are more likely to need preheat than thin HE A flanges.
What should the S355JR certificate show?
The standard and grade, heat number, chemistry including CEV, tensile results from the appropriate location, any ordered impact results at +20 °C, the section designation and the EN 10204 document type. Check that the heat matches the delivered pieces.