LR DH69 steel plate, also written as LR/DH69, LR Grade DH69, Lloyd's Register DH69 or simply DH69 steel plate, is an extra-high-strength, fine-grain structural steel of the Lloyd's Register Rules for Materials (Ch 3, Section 10, high strength steels for welded structures) with 690 MPa minimum yield (t ≤ 50 mm), 770-940 MPa tensile strength and Charpy V-notch toughness at -20°C [-4°F]. In the grade name "D" is the toughness class, "H" means high strength and "69" is the yield level (69 kgf/mm² class, i.e. 690 N/mm²); the IACS UR W16 designation is DH690. Gangsteel, a steel plate exporter, supplies LR DH69 plates in TM or QT condition, cut to size for offshore platforms, jack-up legs and racks, ship structures and other heavy marine steelwork.

Data source: LR Rules for the Manufacture, Testing and Certification of Materials (July 2022), Ch 3 Section 10, Tables 3.10.1-3.10.5, cross-checked with IACS UR W16 Rev.4 Corr.1 (2026). LR states these grades are primarily for marine and offshore structural applications; their use in a ship hull is approved case by case. Verify the current LR edition and the mill approval before ordering.

LR/DH69 Chemical Composition (Heat Analysis), %

 

ElementTMQT
C, max0.160.18
Mn1.00-1.701.70 max
Si, max0.600.80
P, max0.0250.025
S, max0.0150.015
Al total, min0.0200.018
Nb, max0.050.06
V, max0.12*0.12
Ti, max0.050.05
Ni, max2.002.00
Cu, max0.550.50
Cr, max0.501.50
Mo, max0.500.70
N, max0.0250.015
B, max (if added)0.0050.005

Ladle (heat) analysis per LR Rules for Materials Ch 3, Table 3.10.2 / IACS UR W16 Table 1; all listed elements are to be reported. For TM and N/NR steels Nb+V+Ti ≤ 0.26% and Mo+Cr ≤ 0.65% (not applicable to QT). Total Al to N ratio at least 2:1 unless other nitrogen-binding elements are used. Higher Ni may be approved by LR. *TM vanadium: IACS UR W16 Rev.4 gives 0.12% max; the LR 2022 table text is ambiguous on this cell, so the IACS value is shown. Grades at this strength level are supplied only TM or QT (no N/NR route). Neither LR nor IACS UR W16 tabulates separate product (check) analysis limits for these grades, so no product analysis table is given. Values depend on IACS UR W16 / LR Rules for Materials.

LR DH69 Carbon Equivalent (Ceq, CET, Pcm), max %

 

Strength level / conditionCeq, t ≤ 50 mmCeq, 50 < t ≤ 100 mmCeq, 100 < t ≤ 250 mmCETPcm
H69 TM0.56N/AN/A0.360.30
H69 QT0.640.660.700.400.33

Plates, per LR Table 3.10.3 / IACS UR W16 Table 2 (IACS splits the last column into 100-150 and 150-250 mm with the same plate values). Ceq = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15; CET = C + (Mn+Mo)/10 + (Cr+Cu)/20 + Ni/40 (H46 and above, at the manufacturer's discretion); Pcm = C + Si/30 + (Mn+Cu+Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B (TM and QT steels with C ≤ 0.12%). N/A means not applicable. Values depend on IACS UR W16 / LR Rules for Materials.

LR/DH69 Mechanical Properties

 

Propertyt ≤ 50 mm50 < t ≤ 100 mm100 < t ≤ 150 mm
Yield strength ReH, min690 MPa [100 ksi]650 MPa [94 ksi]630 MPa [91 ksi]
Tensile strength Rm770-940 MPa [112-136 ksi]770-940 MPa710-900 MPa [103-131 ksi]

Per LR Table 3.10.4 / IACS UR W16 Table 4 for LR/DH69. Elongation on 5.65√S0: 14% min transverse, 16% min longitudinal. LR additionally limits the actual yield/tensile ratio to 0.94 max unless specially agreed. Where tensile properties must be maintained through the thickness (e.g. offshore racks), no reduction with thickness is permitted.

LR DH69 Elongation on 200 mm Gauge Length (25 mm wide flat specimen)

 

Thickness, mm≤ 1010-1515-2020-2525-4040-5050-70
Elongation, % min9101111121314

Transverse full-thickness specimens, per LR Table 3.10.5 / IACS UR W16 Table 5.

LR DH69 Charpy V-Notch Impact Requirements (-20°C [-4°F])

 

GradeTest temperatureTransverse, avg minLongitudinal, avg min
LR/DH69-20°C [-4°F]46 J69 J

Per LR Table 3.10.4 / IACS UR W16 Table 4: average of three full-size specimens; the same energy applies over the whole thickness range. Plates wider than 600 mm are tested transverse; above 50 mm thickness, specimens are taken at t/4 and additionally at t/2.

Delivery Condition and Deoxidation

LR DH69 is fully killed and fine-grain treated, made to an LR-approved manufacturing specification. Permitted delivery conditions: TM or QT (TM includes TM with accelerated cooling and direct quench + tempering). Vacuum degassing is mandatory at the 690 MPa level. Options by agreement: ultrasonic testing, Z15/Z25/Z35 through-thickness properties (vacuum degassed), and LR survey with 3.2 certificate stating the specified maximum Ceq, CET or Pcm.

Thickness Coverage

Maximum plate thickness: TM 150 mm, QT 150 mm (LR Table 3.10.1); thicker by special consideration. No TM Ceq limit is given above 50 mm, so H69 plates over 50 mm are normally QT. Typical mill sizes are about 8-150 mm thick, 1500-4000 mm wide and 6000-18000 mm long, subject to mill approval.

Equivalent Steel Grades of LR/DH69

 

Society / standardEquivalent grade
IACS UR W16DH690
ABSABS DQ70
CCSD690 (DH690)
GL / DNV / BV / RINAD690
NK / KRKD70 / RD70
ASTM A131no equivalent (A131 stops at 390 MPa)

All IACS members apply UR W16, so chemistry and properties are equivalent, but each plate needs a certificate from the vessel's or structure's own society; dual certification is possible when each surveyor witnesses the tests.

FAQ about LR DH69 Steel Plate

What is LR DH69 steel plate?

An extra-high-strength fine-grain structural steel to LR Rules for Materials Ch 3 Section 10 (IACS UR W16 grade DH690), with 690 MPa minimum yield, 770-940 MPa tensile strength and Charpy testing at -20°C [-4°F].

What does DH69 mean?

D is the toughness class (A 0°C, D -20°C, E -40°C, F -60°C), H means high strength and 69 is the yield level in kgf/mm², i.e. 690 N/mm².

What is the yield strength of LR DH69?

690 MPa min up to 50 mm, 650 MPa for 50-100 mm and 630 MPa for 100-150 mm. Tensile strength is 770-940 MPa up to 100 mm and 710-900 MPa above.

What are the impact requirements for LR DH69?

Charpy V-notch at -20°C [-4°F] with an average of at least 46 J transverse or 69 J longitudinal, for all thicknesses.

What is the maximum carbon equivalent for LR DH69?

For plate up to 50 mm, Ceq max is 0.56 (TM), 0.64 (QT); limits rise with thickness as tabulated above.

How is LR DH69 delivered?

TM or QT, fully killed and fine-grain treated, within the thickness limits of LR Table 3.10.1 and the mill's LR approval.

What is the difference between LR DH69 and LR EH69?

Same strength level; LR DH69 is impact tested at -20°C [-4°F] while LR EH69 is tested at -40°C [-40°F]; the E/F classes also have lower P and S limits.

What is LR DH69 equivalent to?

ABS DQ70, CCS D690, GL D690, DNV D690, BV D690, RINA D690, NK KD70 and KR RD70 (IACS DH690). ASTM A131 has no equivalent at this strength.

Is LR DH69 weldable?

Yes, with qualified procedures and LR-approved consumables of grade 3Y69 or higher (LR Rules for Materials Table 11.1.1); preheat is set from Ceq/CET or Pcm, thickness and restraint.

Other LR Steel Plate Grades

Ordinary and higher-strength grades (235-390 MPa): LR Grade A steel plate | LR Grade B steel plate | LR Grade D steel plate | LR Grade E steel plate | LR AH32 steel plate | LR AH36 steel plate | LR AH40 steel plate | LR DH32 steel plate | LR DH36 steel plate | LR DH40 steel plate | LR EH32 steel plate | LR EH36 steel plate | LR EH40 steel plate | LR FH32 steel plate | LR FH36 steel plate | LR FH40 steel plate

Extra-high-strength 420-500 MPa: LR AH42 steel plate | LR AH46 steel plate | LR AH50 steel plate | LR DH42 steel plate | LR DH46 steel plate | LR DH50 steel plate | LR EH42 steel plate | LR EH46 steel plate | LR EH50 steel plate | LR FH42 steel plate | LR FH46 steel plate | LR FH50 steel plate

Extra-high-strength 550-690 MPa: LR AH55 steel plate | LR AH62 steel plate | LR AH69 steel plate | LR DH55 steel plate | LR DH62 steel plate | LR EH55 steel plate | LR EH62 steel plate | LR EH69 steel plate | LR FH55 steel plate | LR FH62 steel plate | LR FH69 steel plate

Equivalent Class Society Grades

LR DH69 corresponds to the same grade under the other IACS member classification societies: CCS D690 steel plate, ABS DQ70 steel plate, GL D690 steel plate, DNV D690 steel plate, BV D690 steel plate, NK D70 steel plate, KR D70 steel plate, RINA D690 steel plate. ASTM A131 does not cover the 420-690 MPa extra-high-strength levels, so there is no A131 equivalent.

Other Products