ABS Steel Plate
ABS FH36 Steel Plate – Properties, Chemistry & Equivalents

ABS FH36 (also written AB/FH36, ABS Grade FH36, ABS/FH36, FH36 steel plate) is a higher-strength hull structural steel plate to ABS Rules Part 2, Chapter 1, Section 3. The figure 36 is the strength class (minimum yield 355 MPa, tensile 490-620 MPa) and the letter F sets the Charpy V-notch test temperature of -60°C. It is killed and fine-grain treated, with Nb, V, Ti or Al used as grain refiners, and corresponds to grade F36 in IACS UR W11 and FH36 in ASTM A131.
Related grades: ABS AH36 steel plate ABS DH36 steel plate ABS EH36 steel plate ABS FH32 steel plate.
Gangsteel is specialized in supplying ABS high strength steel plate in ABS Grade FH36. For more ``information of GradeFH36 steel plate, please check them in following:
AB/FH36 high Strength Chemical Composition
| Element | Heat analysis (max/min) | Product analysis |
|---|---|---|
| C | ≤ 0.16 | ≤ 0.20 |
| Mn | 0.90–1.60 | 0.81–1.72 |
| Si | 0.10–0.50 | 0.04–0.56 |
| P | ≤ 0.025 | ≤ 0.035 |
| S | ≤ 0.025 | ≤ 0.035 |
| Al (acid-soluble) | ≥ 0.015 | — (no tolerance in ASTM A6 Table A; product value not given) |
| Nb | 0.02–0.05 | 0.010–0.060 |
| V | 0.05–0.10 | 0.040–0.110 |
| Ti | ≤ 0.02 | ≤ 0.03 |
| Cu | ≤ 0.35 | ≤ 0.38 |
| Cr | ≤ 0.20 | ≤ 0.24 |
| Ni | ≤ 0.80 | ≤ 0.83 |
| Mo | ≤ 0.08 | ≤ 0.09 |
| N | ≤ 0.009 (≤ 0.012 if Al present) | ≤ 0.014 |
Al, Nb and V minima apply when used singly (combined minima per ABS 2-1-3/5); Si min does not apply where acid-soluble Al ≥ 0.015%; AH ≤ 12.5 mm may have Mn min 0.70%. N product value shown for the 0.009% limit; with Al present the limit is 0.012% (product ≤ 0.017). Product analysis = heat limit ± ASTM A6/A6M Table A permitted variation (band chosen by the specified maximum/upper limit); applies only when product (check) analysis is required; for a range, results may not vary both above and below it. Per ABS Rules for Materials and Welding Part 2 (2022); product analysis tolerances per ABS 2-1-2/5.3 (“chemical tolerances of ASTM A6”) and ASTM A6/A6M 7.2, Table A (also invoked by ASTM A131). Heat limits: ABS 2-1-3/7.3 Table 1 (t ≤ 150 mm).
Crack Sensitivity: Pcm = (C+Si/30+Mn/20+Cu/20+Ni/60+Cr/20+Mo/15+V/10+5B)%
Carbon Equivalent: Ceq = 【C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15】%
AB/FH36 high strength property
| Thickness (mm) | Yield min (MPa) | Tensile (MPa) | Elongation A5 min (%) | Charpy test temp (°C) | Impact avg min, longitudinal (J) | Impact avg min, transverse (J) |
|---|---|---|---|---|---|---|
| t≤50 | 355 | 490-620 | 21 | -60 | 34 | 24 |
| 50<t≤70 | 355 | 490-620 | 21 | -60 | 41 | 27 |
| 70<t≤100 | 355 | 490-620 | 21 | -60 | 50 | 34 |
Source: ABS Rules Pt 2, 2-1-3 Tables 2 & 4. Either direction acceptable.
Boiler steel plates| Alloy steel plates| High strength plate| Carbon steel plate
|
Equivalent steel grade of AB/FH36 |
|||||||
If you need more stock steel plates in shipbuilding steel plate, please click warehouse sizes.
Related steel grades: AB/E, AB/FH32, AB/FH40, AB/FQ43
|
General Strength |
||||
|
High Strength |
||||
|
Extra Strength |
||||
ABS FH36 thickness and impact requirements
ABS impact energy rises with plate thickness. ABS FH36 is tested at -60°C. Minimum average energies (full-size specimens):
- t≤50 mm: 34 J longitudinal / 24 J transverse
- 50<t≤70 mm: 41 J longitudinal / 27 J transverse
- 70<t≤100 mm: 50 J longitudinal / 34 J transverse
The ABS tables cover plates up to 150 mm. Plates thicker than 100 mm, or produced from coil, have extra rules in ABS Part 2, Chapter 1, Section 1.
| Standard / society | Equivalent grade |
|---|---|
| ABS | AB/FH36 |
| IACS UR W11 | F36 (also written FH36) |
| ASTM A131 | FH36 |
| DNV | VL F36 |
| LR / BV / CCS / RINA | FH36 |
| NK | KF36 |
| KR | RF36 |
Grades are equivalent in chemistry and properties because the IACS societies use the same unified requirements. A plate still needs a certificate from the vessel's own classification society, so one plate can carry dual or multiple class certification only when each society's surveyor tests it.
FAQ
What does FH36 mean?
The letter F sets the Charpy test temperature (-60°C), and 36 is the strength level: minimum yield 355 MPa.
What are the mechanical properties of ABS FH36?
Minimum yield 355 MPa, tensile strength 490-620 MPa and minimum elongation 21%. Charpy average at -60°C is at least 34 J longitudinal / 24 J transverse for t ≤ 50 mm.
What is the impact test temperature of ABS FH36?
-60°C.
What is ABS FH36 equivalent to?
ASTM A131 FH36, IACS UR W11 grade F36, DNV VL F36, and FH36 under LR, BV, CCS and RINA (NK KF36, KR RF36). The plate still needs a certificate from the vessel's classification society.
What is the chemical composition of ABS FH36?
C ≤ 0.16%, Mn 0.90-1.60%, Si 0.10-0.50%, P and S ≤ 0.025%, and at least one grain refiner (Al ≥ 0.015%, Nb 0.02-0.05% or V 0.05-0.10%). Ni ≤ 0.80%.
How is ABS FH36 supplied?
Depending on thickness and grain refiner: as rolled (thin plates of A and D grades only), normalized, controlled rolled or thermo-mechanically rolled; E and F grades are normalized or TM (QT also allowed for 40 grades). See ABS 2-1-3 Table 5.
ASTM equivalent: ASTM A131 FH36 steel plate
LR equivalent: LR FH36 steel plate
-
ABS Grade A Plate – Propertie
ABS Grade A ordinary-strength hull plate: chemical composition, 235 MPa yield, 400-520 MPa tensile, Charpy test
-
ABS EH36 Steel Plate – Proper
ABS EH36 higher-strength ship plate: 355 MPa min yield, 490-620 MPa tensile, Charpy at -40°C, chemistry table
-
ABS DH36 Steel Plate – Proper
ABS DH36 higher-strength ship plate: 355 MPa min yield, 490-620 MPa tensile, Charpy at -20°C, chemistry table
-
ABS AH36 Steel Plate – Proper
ABS AH36 higher-strength ship plate: 355 MPa min yield, 490-620 MPa tensile, Charpy at 0°C, chemistry table an